apollo experience report the problem of stress-corrosion cracking
Post on 09-Apr-2018
213 Views
Preview:
TRANSCRIPT
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
1/23
NASA TECHNICAL NOTE
P_I
Zq4Z
C , :t_C @P-J* ._::_
NASATN D-7111
APOLLO EXPERIENCE REPORT-THE PROBLEM OFSTRESS-CORROSION CRACKING
by Robert E. JohnsonManned Spacecraft CenterHouston, Texas 77058NATIONAL AERONAUTICS AND SPACE ADMINISTRATION WASHINGTON, D. C. MARCH 1973
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
2/23
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
3/23
!1. Report No. I 2. Government Accession No.NASA TN D- 7111 I
4. Title and SubtitleAPOLLO EXPERIENCE REPORTTHE PROBLEM OF STRESS-CORROSION CRACKING
7. Author(s)
Robert E. Johnson, MSC9. Performing Organization Name and AddressManned Spacecraft CenterHouston, Texas 77058
12. Sponsoring Agency Name and AddressNational Aeronautics and Space AdministrationWashington, D.C. 20546
3. Recipient's Catalog No.
5. Report DateMarch 1973
6. Performing Organization Co'de
8. Performing Organization Report No.MSC S-344
10. Work Unit No,914-13-20-06-72
11. Contract or Grant No.
13. Type of Report and Period CoveredTechnical Note
14. Sponsoring Agency Code
15. Supplementary NotesThe MSC Director waived the use of the International System of Units (SI) for this ApolloExperience Report because, in his judgment, the use of SI Units would impair the usefulnessof the report or result in excessive cost.
16, Abstrac t
Stress-corrosion cracking has been the most common cause of structural-material failures inthe Apollo Program. The frequency of stress-corrosion cracking has been high and the magni-tude of the problem, in terms of hardware lost and time and money expended, has been signifi-cant. In this report, the significant Apollo Program experiences with stress-corrosioncracking are discussed. The causes of stress-corrosion cracking and the corrective actionsare discussed, in terminology familiar to design engineers and management personnel, toshow how stress-corrosion cracking can be prevented.
17. Key Words {Suggested by Author(s}) Stress Corrosion Aluminum Alloys Titanium Alloys
18. Distribution Statement
19. Security Classif. (of this report) 20. Security Classif. (of this page) 21. No. of Pages 22. PriceNone None 20 $3.00
* For sale bythe National Technical Information Service, Springfield, Virsinia 2215l
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
4/23
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
5/23
CONTENTS
Section Page
SUMMARY ..................................... 1
INTRODUCTION .................................. I
DISCUSSION .................................... 2
Lunar Module Stress-Corrosion Failures ................... 2
Pressure-Vessel Stress Corrosion ...................... I0
CONCLUDING REMARKS ............................. 14
REFERENCES ................................... 15
iii
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
6/23
FIGURES
Figure12
34
10
11
12
13
Lunar module structure .........................Crack in a swaged type 7075-T6 aluminum tube found on LTA-3
(magnification: 3x) ..........................Closeup of the crack shown in figure 2 (magnification: 7x) ......Edge view of the crack shown in figures 2 and 3 (magnification: 3x).Cross sections of points A_ B_ and C are shown in figure 5 .....Closeups of the cross-section points indicated in figure 4(a) Cross-section point A ........................(b) Cross-section point B ........................(c) Cross-section point C ........................Crack in a typical swaged type 7076-T6 aluminum tube
(magnification: 10x) .........................Cross section of the crack shown in figure 6. The outlined area is
thought to be a swaging lap. Closeup of the outlined area isshown in figure 8 ...........................
Closeup of the outlined area shown in figure 7 .............Significance of gap-dimension errors on the resulting stress(a) Linear offset .............................(b) Angular offset ............................Crack in the radius of a machined longeron made of type 7079-T652
aluminum alloy ............................Crack in the radius of a machined tank-truss fitting made oftype 7075-T6511 aluminum alloy ...................
Crack in the radius of a stiffener made of type 7075-T6 aluminumalloy
(a) Location of the crack in the radius of a stiffener (indicated bydashed line) ...... ... .. ... ... ... .. ... ...
(b) Closeup of the crack shown in figure 12(a) ..... ........Interrivet cracking on a channel made of type 7075-T651 aluminumalloy ..................................
Page3
455
7
iv
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
7/23
Figure14
15
16
17
18
19
Cracking around the fastener holes as a function of the alloygrain direction ................... .........Cracking on a strap made of type 7075-T6 aluminum alloy. The
failure origin can be seen at point A, and secondary cracks canbe seen at points B and C ......................Intergranular cracking at the midthickness from stress-corrosion
cracking and transgranular cracking at surfaces, which indicateshigh tension loads (magnification: 100x) ..............Cracking on a machined part. (Note the relationship of the crackto the alloy grain direction. ) .....................Stress corrosion of type 6A1-4V titanium alloy from a failed nitrogentetroxide pressure vessel(a) Failed pressure vessel .......................(b) Magnified view of the inside surface shorting cracks .......(c) Transgranular cracks .......................(d) Electron fractograph of the failed surface .............(e) Cross section of the pressure-vessel wall showing a flat frac-ture with a shear lip .......................Origin of the failure that resulted from methanol in a type
6A1-4V titanium-alloy pressure vessel(a) Tank cross section at the fracture face (magnification: 10x) .(b) Microstructure of the tank inner surface
(magnification: 50x) .......................(c) Microstructure at the fracture face ................(d) Microstructure at the fracture face (different location fromfig. 19(c)) .............................
Page
I0
1111111112
13131313
V
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
8/23
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
9/23
APOLLO EXPERIENCEREPORTTHE PROBLEMOF STRESS-CORROSION CRACKING
By Robert E. JohnsonManned Spacecraft Center
SUMMARY
Stress-corroSion cracking has been the most common cause of structural-material failures in the Apollo Program. The frequency of stress-corrosion crackinghas been high and the magnitude of the problem, in terms of hardware lost and timeand money expended, has been significant. In this report, the significant Apollo Pro-gram experiences with stress-corrosion cracking are discussed. The causes of stress-corrosion cracking and the corrective actions are discussed, in terminology familiar todesign engineers and management personnel, to show how stress-corrosion crackingcan be prevented.
The basic conclusion of this report is that the environments and alloys used inthe Apollo Program in which failures occurred were generally the same as those en-countered in past aircraft and missile failures. Two exceptions to this conclusion arethe methanol-titanium and the nitrogen tetroxide-titanium incompatibilities, which werecombinations unique to the Apollo Program. Better communications are needed be-tween designers and fabrication personnel, and a more thorough education on existingknowledge of stress-corrosion problems should significantly reduce problems in theconstruction of future spacecraft. A secondary conclusion presented in this report isthat the use of certain aluminum alloys and high-strength steels and the use of certainheat-treatment procedures should be avoided.
I NTRODUCTION
The following definition of stress-corrosion cracking is found in reference 1."When certain metal alloys are exposed to a corrosive environment while at the sametime they are subjected to an appreciable, continuously maintained, tensile stress,rapid structural failure can occur as a result of stress corrosion. This is known asstress-corrosion cracking and is characterized by a brittle type failure in a materialthat is otherwise ductile. "
The stress-corrosion susceptibility of an alloy is affected by the temperature, thegrain direction (in certain alloys), the grain size, and the distribution of phases or pre-cipitates in the alloy, in addition to such obvious factors as alloy composition, environ-ment, and stress level. Although the problem of preventing stress-corrosion cracking
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
10/23
is difficult, the use of correct assemblyproceduresand the proper recognition duringthe designphaseof the factors affecting structural sensitivity canbe instrumental inavoiding this problem.The structural materials used in the Apollo spacecraft hardwareare high-strengthalloys that are widely used in aircraft construction. The stress-corrosion behavior ofthesealloys is well establishedin certain environments. Therefore, it is important
to examinesomeof the Apollo Program hardware failures to determinewhy they oc-curred andhowtheywere overcome.The photographsandmuchof the information in this report were supplied by twoprime Apollo contractors, North American Rockwell andGrummanAerospaceCorpora-tion. The help furnished by theseorganizations in preparing this report is acknowledgedandappreciated.
DISCUSSION
Lunar Module Stress-Corrosion FailuresTo provide a background for the discussion of lunar module (LM) stress-
corrosion failures, a brief description of the LM structure and the design philosophythat affected the stress-corrosion susceptibility of the structure is presented. The LMstructure (fig. 1) is constructed largely of high-strength aluminum alloys along withsmaller amounts of titanium alloys and stainless steels. The evolution and design ofthe LM structure was based on a minimum-weight requirement. After the originaldesign release, two additional weight-reduction programs were conducted to trim everypossible ounce from all structural components. As a result, complex machining ofcomponents from bar stock or plate was combined with chemical milling to achieve ahighly efficient structure from a weight standpoint. However, this approach led to un-desirable stress-corrosion-resistance conditions because of the undesirable graindirections exposed to environments and the sustained high fabrication or residualstresses in the parts.
The first significant failure of an LM structural component was reported inOctober 1967 on an LM test article (LTA-3). A crack was found in a web splice platemade of type 7075-T651 aluminum alloy. The cause of the failure was listed as thehigh installation stresses to which the component was subjected because of the omissionof a shim stock, contrary to the drawing requirements. The stresses, combined withthe water used in the pressure testing of the ascent stage, led to stress-corrosioncracking of the component. Because the failure was attributed to a fabrication errorthat had been complicated by the nature of the test (hydrostatic), no serious thought wasgiven at the time to the possibility that the failure was indicative of a general problem.Unfortunately, subsequent failures proved otherwise.
In December 1967, during the inspection of the same test article, numerous tubesthat were used to support equipment racks were found to be cracked near fasteners orattachment points. This finding led to an examination of other vehicle parts that had a
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
11/23
Figure 1.- Lunar modulestructure.similar construction. Manycomponentsof assembledvehicles andsubassembliessub-sequentlywere found to be cracked. Becausethe failure modesandcauseswere simi-lar, only one representative casewill be described.
The support tubes in the LM aft-equipment-bay assembly (fig. 1)are madeoftype 7075-T6aluminum alloy, andthe endsof the tubesare reduced in diameter byswagingandare attachedmechanically to endfittings. The incidence of cracks at theswagedendsof the tubeswas high (over 20cracked parts) andhad resulted from abuildup of tolerances betweenthe tubeand the fitting. Whentheparts were assembled,sustainedhigh tensile stresses were introduced in the tube, and cracks developedper-pendicular to the direction of high residual stress. In this exampleand in manyother
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
12/23
,'cases, moist air was the environmental factor that caused stress-corrosion cracking.The type of cracking observed and the general locations of the cracks are shown infigures 2 to 8.
Figure 2.- Crack in a swagedtype 7075-T6 aluminum tubefound on LTA-3 (magnifica-tion: 3).
Figure 3.- Closeup of the crack shownin figure 2 (magnification: 7).
Figure 4.- Edge view of the crack shownin figures 2 and 3 (magnification: 3x).Cross sections of points A, B, and Care shown in figure 5.
L_ I(a) Cross-section point A.
Figure 5.- Closeups of the cross-section points indicated infigure 4.
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
13/23
F- -7
(c) Cross-section point C.
Figure 5. - Concluded.
(b) Cross-section point B.
Figure 6. - Crack in a typical swagedtype 7075-T6 aluminum tube(magnification: 10x).
Figure 7. - Cross section of the crackshown in figure 6. The outlined areais thought to be a swaging lap.Closeup of the outlined area is shownin figure 8.
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
14/23
Figure 8. - Closeup of the outlined areashown in figure 7.
\
To eliminate the problem, allsuch fittings on assembled vehicleswere disassembled; the gaps createdby the tolerances in the mating partswere filled by means of liquid shim-ming, a technique by which a room-temperature-curing resin wasintroduced into the volume betweenthe parts and allowed to harden be-fore the parts were joined perma-nently by mechanical fasteners.
The discovery of the numerousfailures alerted the contractors andNASA to the possibility that stressesintroduced by the assembly tech-niques used by the contractor easilycould cause stress-corrosion crack-ing on other parts of assembled ve-hicles. Because the time at whichstress-corrosion cracking occurscan vary, often occurring after long
periods of time, all susceptible alloys on all LM vehicles were suspect. Therefore,hardware designs that involved type 7075, 7079, 2014, 2024, and 7178 aluminum alloyswere examined to evaluate the design and assembly stresses and to identify the locationsat which sustained stresses were of a sufficient magnitude to cause stress-corrosioncracking. During the design review, approximately 1000 parts were judged to be sus-ceptible to stress-corrosion cracking, approximately 500 design components were listedas probable problems that would require detailed analysis, and approximately 170 partswere found to constitute possible problems.
To examine these potential problems, representatives of the contractor, the NASAManned Spacecraft Center and Marshall Space Flight Center, and the U.S. Air Forceand Navy reviewed the acceptance criteria to be used in the detailed analyses. The con-tractor and NASA began a review of design drawings, and vehicle inspections were con-ducted that revealed additional cracked parts and other critical parts that requiredredesign.
During the investigation, it was noted that many cracked parts failed because ofthe improper fitting of mated parts, particularly where angles or channels nested to-gether and were fastened by bolts or rivets. The process by which stresses can reachthe threshold required for stress-corrosion cracking (8000 psi or higher, depending onthe type of alloy and the alloy grain direction relative to the stress) is shown in figure 9.If proper precautions in the mating and shimming are not taken to eliminate the gap,high stresses can occur, particularly in the radius along the length of the parts. Ex-amples of this type of problem are shown in figures 10 to 12.
Another type of cracking often observed was cracking between such fasteners asrivets or bolts. This type of cracking usually resulted from poor preparation of theholes (burrs, lips, etc. ) and was aggravated by expanded rivets, which increased thestresses around the fastener holes. Examples of these failures are shown in figures 1 3and 14.
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
15/23
77JJIJt/I
0.040 in., constant"----0.375 in.
F ffff ff_l_ | ' ,Gapsize, in. Stress, psi -J Gapsize, in.
O.002 18000 O.002O.005 54000 O.006
(a) Linear offset.
040 in., constant
L_Stress, psi I9 00027000
(b) Angular offset.Figure 9.- Significance of gap-dimension errors on the resulting stress.
%
Crack
Figure 11.- Crack in the radius of amachined tank-truss fitting madeof type 7075-T6511 aluminumalloy.
Figure 10.- Crack in the radius of a ma-chined longeron made of type 7079-T652aluminum alloy.
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
16/23
(a) Location of the crack in the radius (b) Closeup of the crack shown inof a stiffener (indicated by figure 12(a).dashed line).
Figure 12. - Crack in the radius of a stiffener made of type 7075-T6 aluminum alloy.
F- 7
L_ JFigure 13.- Interrivet cracking on a channel made of type 7075-T651 aluminum alloy.
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
17/23
Still anothertype of failure involved straps. The clamping of parts resulted insustainedhigh stresses, which in somecaseswere quite close to the tensile yieldstrength. An exampleof this type of failure is shownin figures 15and 16.Complexparts that are machinedfrom thick sections and in which short trans-verse loads are possible are particularly vulnerable to cracking becausestress-corrosion-cracking threshold stresses are lowest in the transverse direction. Anexample is shownin figure 17. 7
L_ .__LFigure 15.- Cracking on a strap made oftype 7075-T6 aluminum alloy. Thefailure origin can be seen at point A,and secondary cracks can be seen atpoints B and C.
LFigure 14. - Cracking around thefastener holes as a function ofthe alloy grain direction.
/L AFigure 16.- Intergranular cracking atthe midthickness from stress-corrosion cracking and transgranularcracking at surfaces, which indicateshigh tension loads (magnifica-tion: 100x).
9
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
18/23
[- -3 Over 130 parts in the LM programwere found to be cracked as a result ofstress corrosion. Many corrective actionswere instituted. Among the solutions werecomponent redesign, heat treatment to makethe components less susceptible, shimmingor otherwise relieving fabrication stresses,addition of corrosion-protection coatings topreclude as much of the corrosive environ-ment as possible, and shot peening to in-troduce compressive surface stresses.
Pressure-Vessel Stress Corrosion
L_ _3Figure 17. - Cracking on a machinedpart. (Note the relationship of thecrack to the alloy grain direction. )
The problem of stress-corrosioncracking in pressure vessels is especiallyserious because the occurrence of this prob-lem usually results in catastrophic failure ofthe vessel and associated damage to otherhardware near the pressure vessel. Someof the significant Apollo Program pressure-vessel failures are described individuallyin the following sections.
Nitrogen tetroxide in titanium-alloypressure vessels.- In all of the Apollospacecraft propulsion systems, nitrogentetroxide is used as the oxidizer. The stor-age of nitrogen tetroxide under pressure intitanium-alloy pressure vessels was a sub-ject of concern because of known reactionsbetween titanium and other oxidizers. Ex-tensive test programs were conducted before1964 to approve the use of type 6A1-4V tita-nium alloy as the standard Apollo space-
craft pressure-vessel material for this application. In 1964, qualification tests on theApollo spacecraft main propellant tanks were completed. The tests included 30-dayexposures of the pressure vessels to nitrogen tetroxide under the maximum wall stressof approximately 100 ksi.
In 1965, a stress-corrosion failure of an Apollo reaction control system pressurevessel occurred. This failure could only have been caused by the nitrogen tetroxidereacting with the titanium-alloy pressure vessel. The failure analysis (refs. 2 and 3)showed that a change in the nitrogen tetroxide composition, within the limits of the pro-curement specification for the oxidizer, had eliminated one oxide of nitrogen and createda fluid that was causing serious stress-corrosion cracking of the titanium alloy. De-tails of the failed hardware are shown in figure 18.
10
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
19/23
V- 7
IL __J(a) Failed pressure vessel.
W-
L_(b)
f ( ;1 ,,
i; , J
t ii
!
't;t
JMagnified view of the inside surface
showing cracks.
V-- -]"A
L J L J(c) Transgranular cracks. (d) Electron fractograph of the failedsurface.
Figure 18.- Stress corrosion of type 6A1-4V titanium alloy from a failed nitrogentetroxide pressure vessel.
11
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
20/23
r-
1
-1
_A(e) Cross section of the pressure-
vessel wall showing a flatfracture with a shear lip.Figure 18.- Concluded.
To eliminate the problem, NASA gen-erated a nitrogen tetroxide procurementspecification that carefully controlled theoxidizer composition to maintain compati-bility with the pressure-vessel titaniumalloy. In addition, by taking samples of theoxidizer from the flight supply system be-fore the oxidizer is loaded into the space-craft and by testing the oxidizer in contactwith stressed precracked samples of thepressure-vessel alloy, NASA continues toensure that no fluid change has occurredthat could cause aggressive reactions dur-ing a flight.
Methanol in titanium-alloy pressure vessels. - The most damaging failure of apressure vessel in the Apollo Program occurred in October 1966 when a main propel-lant tank ruptured inside an Apollo service module and caused extensive damage andserious loss of hardware. The failure occurred while the pressure vessel, made oftitanium alloy 6A1-4V, was filled with methanol and was pressurized. The failure modewas stress-corrosion cracking.
In this instance, methanol was used for safety reasons in the system checkout in-stead of the toxic propellant. Methanol was selected for its physical similarity (density,viscosity) to the propellant and because it could be removed from the system easilywithout leaving a residue or other contamination. The approval for the use of methanolwas based on a literature search, which uncovered no data to indicate a potential prob-lem. After the failure of the Apollo spacecraft hardware, numerous programs wereinitiated to investigate the problem, and the seriousness of the problem was defined inseveral technical papers (ref. 4). Examples of the metallography from the failed mate-rial are shown in figure 19. Additional information concerning the failure analysis iscontained in references 3 and 5.
In retrospect, the lack of a test program to approve pressure-test fluids beforethey were used and a continuing check against contaminants during use caused a seriousprogram problem. The Manned Spacecraft Center has corrected this situation by re-quiring compatibility testing before a new pressure-vessel material or a new test en-vironment can be used in the Apollo Program.
12
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
21/23
...........awCut
...........a)..""
o..*
Tallk cross section at the fractureface (magnification: 10"/
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking
22/23
two motor cases. The test fluid was water, andfailure analysis showedthat stress-corrosion cracking would occur if defects existed in thestressedalloy whenit wasbrought into contact with water. The defectsin the motor caseswere identified astight cracks that hadresulted from the welding operation andthat could not be detectedby the postweldinspection. The corrective action for the problem was to changeto acompatible test fluid, hydraulic fluid, andto makethe inspectionandquality-controlprocedures of the welding operation more thorough.Oxygen-storage vessel made of type D6AC steel alloy. - Type D6AC steel alloy
was heat treated to the 220 000- to 240 000-psi tensile-strength range and was used tostore gaseous oxygen under pressure. The failure of one pressure vessel because ofstress-corrosion cracking was caused by a small defect on the exterior surface of thepressure sphere. The corrosive medium was listed as water because the test consistedof immersing the vessel under water during hydrostatic testing. The vessel was nickelplated and the defect was found to contain nickel, which indicated the presence of theflaw before nickel plating. The corrective action taken was to change the test fluid tooil and to discontinue the immersion of the tank during pressure testing. Also, inspec-tion procedures were tightened to enable detection of pressure-vessel defects beforetesting.
C ONC L USIONS
The Apollo spacecraft is constructed of high-strength alloys and is designed andfabricated to be a highly efficient, low-weight vehicle. Stress corrosion has been a se-rious problem in the Apollo Program and reflects the type of problem that can occurin a program requiring these characteristics. To illustrate the type of problem en-countered, several examples are examined.
The examples discussed in this report are typical ones and do not represent allof the stress-corrosion cracking failures experienced in the Apollo Program. How-ever, the examples discussed do represent the most significant problems encounteredin the Apollo Program and allow the following general conclusions to be drawn concern-ing improvements that are needed to prevent the recurrence of similar problems infuture programs.
1. With the exception of two environments, information on the stress-corrosioncracking behavior of the alloys used in Apollo spacecraft hardware was available andcould have been used to avoid many of the stress-corrosion cracking failures if the in-formation had been applied correctly during the design, fabrication, and test phases.
2. Without proper consideration of stress-corrosion cracking, such designchanges as those for vehicle weight reduction can seriously affect the stress-corrosionsensitivity of the vehicle hardware by changing fabrication techniques, raw-materialmill forms, and stress levels, and by eliminating corrosion-protection systems.
3. Specific alloys and alloys subjected to certain heat-treatment procedures arevery susceptible to stress-corrosion cracking, and their use should be avoided wher-ever possible. Control should be exercised by the contractors and NASA over the use
14
-
8/8/2019 Apollo Experience Report the Problem of Stress-Corrosion Cracking