    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    1

    Casting Processes

    ver. 2

  • 5/19/2018 casting defects and process

    2/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    2

    Types of Parts Made

    Engine blocks

    Pipes

    Jewelry

    Fire hydrants

  • 5/19/2018 casting defects and process

    3/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    3

    Complex, 3-D shapes

    Near net shape

    Low scrap

    Relatively quick process

    Intricate shapes

    Large hollow shapes

    No limit to size Reasonable to good surface finish

  • 5/19/2018 casting defects and process

    4/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    4

    Processes

    Sand

    Shell

    Plaster

    Ceramic Investment

    Lost foam

    Pressure Vacuum

    Die Centrifugal

    Squeeze

    Semi-solid Single crystal

    Directional

    solidification Slush

    Continuous

  • 5/19/2018 casting defects and process

    5/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    5

    Metals processed by casting

    Sand casting60%

    Investment casting7%

    Die casting9%

    Permanent mold casting11%

    Centrifugal casting7%

    Shell mold casting6%

  • 5/19/2018 casting defects and process

    6/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    6

    Breakdown of Castings

    Ingots for bulk deformation processing -

    85%

    Cast to near net shape - 15%

  • 5/19/2018 casting defects and process

    7/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    7

    Ingots

    Iron or steel molds

    Water-cooled molds

    Continuous casting

  • 5/19/2018 casting defects and process

    8/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    8

    Shapes

    Expendable Molds

    sand

    shell slurry

    investment

    lost wax

    lost foam

    Permanent mold

    (cavity)

    die casting hot chamber

    cold chamber

  • 5/19/2018 casting defects and process

    9/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    9

    Shapes

    Centrifugal

    pipes

    spinning

  • 5/19/2018 casting defects and process

    10/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    10

    Capabilities

    Dimensions

    sand casting - as large as you like

    small - 1 mm or so

    Tolerances

    0.005 in to 0.1 in

    Surface finish

    die casting 8-16 micro-inches (1-3 mm)

    sand casting - 500 micro-inches (10-25 mm)

  • 5/19/2018 casting defects and process

    11/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    11

    Casting Stepsquick route from raw material to finished

    product

    Melt metals

    Pour / force liquid into hollow cavity

    (mold)

    Cool / Solidify

    Remove

    Finish

  • 5/19/2018 casting defects and process

    12/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    12

    Melting

    Raw material (charge)

    scrap, alloying materials

    Atmosphere

    Air (oxygen), vacuum, inert gas (argon)

    Heating

    External - electric, gas, oil

    Internal - induction, mix fuel with charge

    steel making in blast furnace -mix coke with iron

    Furnace material

    refractory ceramics

    Heat

    Raw materials

    Furnace

    Atmosphere

  • 5/19/2018 casting defects and process

    13/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    13

    Furnaces

    Blast furnace Basic Oxygen Furnace

  • 5/19/2018 casting defects and process

    14/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    14

    Furnaces

    Electric Arc Furnace

    Oxygen-Fuel,

    Oxygen Lance Furnace

  • 5/19/2018 casting defects and process

    15/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    15

    Furnaces

    Induction Furnace Electric Furnace

  • 5/19/2018 casting defects and process

    16/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    16

    Sand Casting

  • 5/19/2018 casting defects and process

    17/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    17

    Sand Casting

  • 5/19/2018 casting defects and process

    18/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    18

    Sand Casting

  • 5/19/2018 casting defects and process

    19/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    19

    Sand Casting Steps

  • 5/19/2018 casting defects and process

    20/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    20

  • 5/19/2018 casting defects and process

    21/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    21

    Sand Cast Parts

  • 5/19/2018 casting defects and process

    22/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    22

    Permanent Mold Casting

  • 5/19/2018 casting defects and process

    23/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    23

    Low Pressure Casting

  • 5/19/2018 casting defects and process

    24/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011

    24

    Die Casting (high pressure)

  • 5/19/2018 casting defects and process

    25/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 25

    Die Casting Machine

  • 5/19/2018 casting defects and process

    26/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 26

    Die Casting

    Cold chamber

    Hot chamber

  • 5/19/2018 casting defects and process

    27/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 27

    Direct Squeeze Casting

  • 5/19/2018 casting defects and process

    28/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 28

    Die Casting Part Example

  • 5/19/2018 casting defects and process

    29/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 29

    Continuous Casting

  • 5/19/2018 casting defects and process

    30/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 30

  • 5/19/2018 casting defects and process

    31/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 31

  • 5/19/2018 casting defects and process

    32/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 32

  • 5/19/2018 casting defects and process

    33/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 33

    InvestmentCasting

  • 5/19/2018 casting defects and process

    34/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 34

    Vacuum Casting

  • 5/19/2018 casting defects and process

    35/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 35

    Investment (top) and Conventional

    Castings

  • 5/19/2018 casting defects and process

    36/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 36

    Lost Foam Casting

  • 5/19/2018 casting defects and process

    37/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 37

    Lost Foam Castings

  • 5/19/2018 casting defects and process

    38/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 38

    Centrifugal Casting

    verticalsand-lined mold

    casting

    horizontal

  • 5/19/2018 casting defects and process

    39/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 39

    Centrifugal Casting

  • 5/19/2018 casting defects and process

    40/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 40

    Pipe CastingProcess

  • 5/19/2018 casting defects and process

    41/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 41

    Directional Solidification

  • 5/19/2018 casting defects and process

    42/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 42

    Casting CharacteristicsTable 5.6

    Typical Weig ht (kg)

    Typical

    surface

    Section

    thickness (mm)

    Process

    materials

    cast Minimum Maximum

    finish

    (micron,

    Ra) Porosity*

    Shape

    complexity

    *

    Dimensional

    accuracy* Minimum Maximum

    Sand All 0.05 No limit 5-25 4 1-2 3 3 No limit

    Shell All 0.05 100+ 1-3 4 2-3 2 2 --

    Expendable

    mold

    pattern All 0.05 No limit 5-20 4 1 2 2 No limit

    Plaster

    mold

    Nonferrou

    s (Al, Mg,

    Zn, Cu) 0.05 50+ 1-2 3 1-2 2 1 --

    Investment

    All

    (High melting

    pt.) 0.005 100+ 1-3 3 1 1 1 75

    Permanent

    mold All 0.5 300 2-3 2-3 3-4 1 2 50

    Die

    Nonferrou

    s (Al, Mg,Zn, Cu)

  • 5/19/2018 casting defects and process

    43/61

    ME 4210: Manufacturing Processes and EquipmentProf. J.S. Colton GIT 2011 43

    Microstructure

  • 5/19/2018 casting defects and process

    44/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    44

    Microstructure - Dendrites

    Finer structure at

    walls

    Grains / dendrites

    grow to center

  • 5/19/2018 casting defects and process

    45/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    45

    Grains on Willie Bs head

  • 5/19/2018 casting defects and process

    46/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    46

    Microstructure - Dendrites

  • 5/19/2018 casting defects and process

    47/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    47

    Fluidity

  • 5/19/2018 casting defects and process

    48/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    48

    Casting Defects - Porosity

  • 5/19/2018 casting defects and process

    49/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    49

    Casting Defects

  • 5/19/2018 casting defects and process

    50/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    50

    Shrinkage

    TABLE 5.1

    Metal or alloy

    Volumetric

    solidification

    contraction (%) Metal or alloy

    Volumetric

    solidification

    contraction (%)

    Aluminum 6.6 70%Cu30%Zn 4.5

    Al4.5%Cu 6.3 90%Cu10%Al 4

    Al12%Si 3.8 Gray iron Expansion to 2.5

    Carbon steel 2.53 Magnesium 4.2

    1% carbon steel 4 White iron 45.5

    Copper 4.9 Zinc 6.5

    Source: After R. A. Flinn.

  • 5/19/2018 casting defects and process

    51/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    51

    Differential Cooling

    Transition between thicker and thinner

    sections can lead to porosity

  • 5/19/2018 casting defects and process

    52/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    52

    Pipe Defect

    Due to shrinkage giving rise to

    a funnel-like cavity

    Solutions insulate top (glass wool)

    heat top (exothermic mixture -

    thermit)

  • 5/19/2018 casting defects and process

    53/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    53

    Defects - Hot Tears

    Chills

  • 5/19/2018 casting defects and process

    54/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    54

    Chills

  • 5/19/2018 casting defects and process

    55/61

    Car Rims

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    55

    Stamped Cast

  • 5/19/2018 casting defects and process

    56/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    56

    Casting Defects - Porosity

  • 5/19/2018 casting defects and process

    57/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    57

    Design Rules Summary

    Uniform wall thickness Flat parting lines

    Gradual thickness

    transitions

    Draft for removal

    tapers: 0.5 to 2 degrees

    Surface of mold gives

    surface of part

  • 5/19/2018 casting defects and process

    58/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    58

    Sand Casting Rules

  • 5/19/2018 casting defects and process

    59/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    59

    Casting costs

    TABLE 5.10Cost*

    Process Die Equipment Labor Productionrate (Pc/hr)

    Sand L L LM

  • 5/19/2018 casting defects and process

    60/61

    ME 4210: Manufacturing Processes and Equipment

    Prof. J.S. Colton GIT 2011

    60

    Process economics