clinker formation concepts
TRANSCRIPT
-
7/27/2019 Clinker Formation Concepts
1/28
Introduction:
Why study clinker burning?
To understand the influence of changes in kilnoperation conditions
Normal kiln operation
Influence of chemistry, fineness, mineralogychanges
Influence of new mix components (pozzolan,AFR, sand, etc.)
Abnormal kiln operation
know causes of badly burnt clinker
understand why rings and deposits form
be able to suggest counter measures
Synthetic Hydraulic Minerals
Analogy to transformation of igneous and sedimentary rocks
into metamorphic rocks
Difference in T, p, t
-
7/27/2019 Clinker Formation Concepts
2/28
==========================================================================================
=
Two principal steps during transformation into clinker
Disintegration of original structure
Mechanical crushing and grinding
Thermal decomposition
Structural rearrangement on heating (e.g. polymorphism
Formation of new structures
Occurrence of intermediate products
Genesis and growth of final clinker minerals
Crystallization of liquid phase
=============================================
========================================
Features characterising the clinker formation process
-Complex system (series of diverse mechanisms)!
-Requires mechanical, thermal and electrical energy
-Reaction rate is slow (necessity of high temperatures, finely dispersedmaterial)
-Clinker minerals are not stable at normal temperature!
-Quality of product is determined by:
Clinker chemistry
Clinker microstructure
====================================================================================
-
7/27/2019 Clinker Formation Concepts
3/28
Control of burning process
Material technological aspects
-Raw meal burning behaviour
Burnability
Dust formation
Coating behaviour
Granulation of clinker
etc.
-Quantity and properties of liquid phase
Process technological aspects
-Temperature profile
-Kiln atmosphere
-Fuel type
-Flame characteristics
===================================================================================
-
7/27/2019 Clinker Formation Concepts
4/28
Reaction pathway
indicates the intermediate products occurring between reactants and products
Reaction mechanism
type(s) and reaction(s) taking place
Reaction kinetics
indicates rate at which the final products are produced
Reaction thermodynamics dictates whether reaction will be at all possible, and what the heat and
temperature requirements will be
===================================================================
=====================================================
Now to my linkedin colleges I finished the first part of my lectureif you have any question contact me here or in my linkedinaccount
Or contact me by Email :[email protected]
===========================================
======================================================
Reaction Pathways Encountered During Clinker Formation
Basic Sequence of Reactions
Mineralogical and Chemical Characteristics of Raw Mixes
Intermediate Products
Liquid Phase
mailto:[email protected]:[email protected]:[email protected]:[email protected] -
7/27/2019 Clinker Formation Concepts
5/28
The Overall Reaction Sequence
To fully describe the pathway of clinkering, it is necessary to consider
the following aspects:
-the chemical and mineralogical content of the raw mix
-the overall sequence of reactions
-the chemical and mineralogical nature of the intermediate products
Heating (C)
20 100 Evaporation of H2O
100 300 Loss of physically adsorbed water
400 900 Removal of structural H2O (H2O and OH groups) from clay
minerals
>500 Structural changes in silicate minerals
600 900 Dissociation of carbonates
>800 Formation of belite, intermediate products, aluminate and ferrite
>1250 Formation of liquid phase (aluminate and ferrite melt)
~1450 Completion of reaction and re-crystallization of alite and belite
-
7/27/2019 Clinker Formation Concepts
6/28
Cooling (C)
1300 1240Crystallization of liquid phase into mainly aluminate and ferrite
=================================================
===========================================================================
Mineralogical characteristics of raw mixes
Carbonates
MgCO3, ankerite CaCO3 (Mg,Fe)CO3 magnesite MgCO3, siderite FeCO3calcite
CaCO3, dolomite CaCO3
Simple Oxides
quartz SiO2, hematite Fe2O3, magnetite Fe3O4
Feldspars
potassium feldspars (Na,K)Si3O8 and
plagioclase series (Na,Ca)(Si,Al)Al2Si2O8
Sheet silicates
minerals of the mica and chlorite groups
(e.g. biotite, muscovite, chlorite),
clay minerals (e.g. kaolinite, montomorillonite, illite, palygorskite)
Hydroxides
Al-hydroxides (e.g. boehmite),
Fe-hydroxides (e.g. goethite, limonite)
Sulfides / sulfates
H2Opyrites FeS2, anhydrite CaSO4, gypsum CaSO4
Fluorides
fluorspar CaF2
-
7/27/2019 Clinker Formation Concepts
7/28
=================================================
===========================================
=================================================
============================================
Intermediate products encountered during clinker production
Type Mineral Name Formula
Simple Sulfates anhydrite CaSO4
-
7/27/2019 Clinker Formation Concepts
8/28
arcanite K2SO4
Ca SO4Compound Sulfates sulfate-spurrite 2(C2S)
calcium-langbeinite K2Ca2 (SO4)3
CaCO3Compound Carbonates spurrite 2(C2S)
Simple Chlorides sylvite KCl
Al2O3 7 Al2O3CaO Calcium Aluminates mayenite 12 CaO
Calcium Ferrites Fe2O3 2 CaO
SiO2 Al2O3 Calcium Alumino-Silicates gehlenite 2 CaO
==================================================================================================
=======================================
Reasons for the formation of intermediate products
-Intermediate products are preferentially formed by kinetically faster reaction
rates
-Intermediate products are the reaction products of localised zones in the meal
charge,
i.e. local equilibrium but not overall equilibrium was reached (e.g. gehlenite
formation)
-Intermediate products are really the equilibrium products at the given
temperature and gas atmosphere,
but not at the final clinkering temperature (e.g. spurrite formation)
=================================================
=================================================
=====
Liquid Phase
basically created by early melting compounds such as Fe2O3 and Al2O3 and
some minor compounds such as MgO and Alkalis
-
7/27/2019 Clinker Formation Concepts
9/28
The composition of the raw mix determines
-temperature at which liquid will first be formed
-amount of liquid formed at any given temperature
-the physical properties of the liquid at any particular temperature, especially
its viscosity
-Although most raw mixes show about the same minimum temperature of
liquid formation (eutectic point),
the quantity of liquid formed at this and progressively higher temperatures
varies according to the raw mix chemistry.
-In the Portland cement relevant parts of the system C S A F, in which
melting begins at 1338 C, the composition of the liquid is:
CaO - 55 %
SiO2 - 6 % Alumina ratio
Al2O3 - 23 % (AR) = 1.38
Fe2O3 - 16 %
Quantity calculation formulae acc. to LEA, considering different
temperature:
1338 oC = 6.1 Fe2O3 + MgO + Na2O + K2O if AR 1.38
8.2 Al2O3 5.22 Fe2O3 + MgO + Na2O + K2O if AR 1.38
1400 oC = 2.95 Al2O3 + 2.2 Fe2O3 + MgO + Na2O + K2O for MgO 2%
1450 oC = 3.0 Al2O3 + 2.25 Fe2O3 + MgO + Na2O + K2O for MgO 2 %
Quantitative change of liquid phase with temperature in several group
plants (influence of MgO, Na2O and K2O included)
-
7/27/2019 Clinker Formation Concepts
10/28
Influence of Al2O3 and Fe2O3 alone on the quantity of liquid formed at
1338 C.
The most effective use of Al2O3 and Fe2O3 with respect to liquid
formation at 1338 C occurs when the two are used in the weightratio of 1.38
-
7/27/2019 Clinker Formation Concepts
11/28
Viscosity of liquid phase
-The viscosity of the liquid phase diminishes exponentially with increasing
temperature and at 1400 C is reduced by addition of fluxing components in
the following order:
Na2O < CaO < MgO < Fe2O3 < MnO
-With increasing SiO2 content of the melt and to a lesser extent with increasing
Al2O3, appreciable increases in viscosity occur.
=================================================
=================================================
=========================================
The overall reaction sequence, displayed based on qualitative change of
minerals from samples taken from an operational kiln
Minerals identified at different locations (long wet kiln)
Sequence of compound formation according to chemical composition
-
7/27/2019 Clinker Formation Concepts
12/28
==============================================
==============================================
==============================================
========
Now to my linkedin colleges I finished the second part of mylecture if you have any question contact me here or in my linkedinaccount
-
7/27/2019 Clinker Formation Concepts
13/28
Or contact me by Email :[email protected]
=====================================================================================================================
Reaction Mechanisms
Definitions
State of matter
solid: definitive volume and definite shape
liquid: definitive volume, assumes shape of container
gaseous: neither definitive volume nor definite shape
Classification of reactions
1. according to their type:
low quartzstructural change high quartz
CaO + CO2decomposition CaCO3
C2Scombination 2CaO + SiO2
2. according to the state of matter:
belitesolid solid quartz and free CaO
crystallisation of aluminate + ferritesolid liquid liquid phase
CaO + CO2solid gas CaCO3
liquid liquid -
liquid gas drying process, volatilisation of alkalis
CO2gas gas CO + 1/2 O2
3. according to rate controlling step (kinetics of reaction)
mailto:[email protected]:[email protected]:[email protected]:[email protected] -
7/27/2019 Clinker Formation Concepts
14/28
diffusion formation of alite
belite (initial reaction)phase boundary quartz + free CaO
nucleation liquid phase crystallisation of aluminate + ferrite; alite formation
Examples
Structural changes: Arrangement of the atoms in low and high quartz
Structural changes: Calcite Aragonite transition
Decomposition reactions (during clinker production)
-solid / gas type
-
7/27/2019 Clinker Formation Concepts
15/28
De-hydroxylation of the clay minerals (kaolinite, etc.)
De-carbonation of the carbonate minerals (magnesite, dolomite, calcite,
spurrite)
-solid / solid type
decomposition of alite
Characteristic of this reaction type is that the single reactant is transformed
into two products.
=================================================
=================================================
=======================================
Decomposition reaction: Equilibrium dissociation pressure of calcite and
spurrite with temperature
Decomposition reaction: Decomposition of C3S at 1175 C
In the case of impure C3S, i.e. clinker alite, the rate of decomposition is
appreciably accelerated by:
the presence of lime and C2S nuclei the presence of Fe2+ , H2O and K2SO4 /
CaSO4 melts
-
7/27/2019 Clinker Formation Concepts
16/28
Combination reaction: Formation of Belite
Belite formation is the result of a combination between the calcite and silica
components of the raw mix.
The rate limiting mechanism by which belite is formed (after an initial phase
boundary controlled reaction) depends on the diffusion of ions through the
solid state.
The rate of this reaction is thus dependent on:
the path distance that the diffusing species
have to travel
defects in the reactants crystal lattices.
Combination reaction: Formation of Alite
Formation of alite only at T > 1250 C (lower stability limit). At that
temperature, the liquid phase is also starting to form: The formation of alite is
a liquid solid reaction
-
7/27/2019 Clinker Formation Concepts
17/28
The formation of alite and its stabilisation depends on the presence of
the liquid phase.
The rate of reaction is dependent on:
the path distance that the diffusing species
have to travel
quantity and viscosity of liquid phase
====================================================
==========================
==========================
==========================
================
Now to my linkedin colleges Ifinished the third part of my lectureif you have any question contact mehere or in my linkedin account
Or contact me by Email :[email protected]
========================================================================
========================
=====================
4. Kinetics of Clinker Burning
mailto:[email protected]:[email protected]:[email protected] -
7/27/2019 Clinker Formation Concepts
18/28
Theoretical consequences:
Rate increases with higher temperature (but also costs!)
Rate decreases with higher activation energy (different raw mix mineralogy)
Rate increases with higher frequency factor (larger contact surface, i.e. finer
mix)
The rate of reaction
increases with temperature and contactsurface between raw mix components
(frequency factor A)
decreases with higher activation energy Eafor raw mix components.
To compensate for the slow reactivity of the less reactive minerals, a higher
burning temperature and / or longer burning period (longer clinkering zone) is
required.
Practical considerations:
-
7/27/2019 Clinker Formation Concepts
19/28
development of suspension preheater
In practice, the most convenient method offollowing the reaction is by measuring the
rate of decrease of non-combined lime (i.e.
free lime).
This technique is illustrated in the followingfigures that show two raw mixes, I and II,
ofidentical chemistry (LS = 95, SR = 3.2
and AR = 2.2) and similar fineness (R200m
= 0.5 %, R90m = 7 % and R60m = 15 %). It is evident that the difference in
mineralogy and actual particle size of
the individual crystals influence both the
mechanism and rate of reaction, especially
at start of the clinker formation.
-
7/27/2019 Clinker Formation Concepts
20/28
Limestone
Calcite 97 %
Dolomite ~ 2 %
Quartz traces
Chlorite -
Illite and Micas -
Pyrite traces
Feldspars -
Shale A
Calcite ~ 40 %
Dolomite -
Quartz ~ 25 %
Chlorite ~ 20 %
Illite and Micas ~ 10 %
Pyrite ~ 2 %
Feldspars ~ 2 %
Shale S
Calcite ~ 10 %
Dolomite -
Quartz ~ 55 %
Chlorite ~ 10 %
Illite and Micas ~ 20 %
-
7/27/2019 Clinker Formation Concepts
21/28
Pyrite traces
Feldspars traces
==============================================
-
7/27/2019 Clinker Formation Concepts
22/28
==============================================
==============================================
=====
Assessment of Raw Meal Burnability
In practice, simple methods are mostly applied to asses the burnabilityof amix, i.e. the ease of formation of the clinker minerals. Three distinct methods
are practiced at HGRS:
Statistical burning model in which ten material parameters influence the rate
of clinker formation. The non-combined CaO value, of any raw mix, relative to
that of a standard raw mix is calculated.
Physicochemical burning model requires no standard raw mix. Only 4
parameters need to be considered.
=================================================
=================================================
===============================================
Statistical Burnability Model
Quantitative evaluation of the data obtainedby the Mark burnability test
o The 1350, 1400 and 1450 free limevalues of other raw mixes from the
same raw material components can be
determined based on one single
burnability test of one mix
o Chemical Parameters: limesaturation, silica ratio, alumina ratio,
K2O + Na2O, MgOo Physical Parameters: residue on 200
m and 90 m sieves, quantity of
mica, quartz and iron minerals
NOTE : The burnability model can be used as an instrument for optimization of
raw mixes
=================================================
==================================================================================================
=
-
7/27/2019 Clinker Formation Concepts
23/28
Physiochemical Burnability Model
the amount of uncombined lime depends ono Specific reaction area (area of contact
between grains)
o Local oversaturation (grain size ofindividual minerals)
o Ambient conditions (pressure,temperature, burning time)
o Diffusion coefficient of CaO through theliquid phase (composition of the liquid
phase)
o Amount of liquid phase formed duringburning
o Supply and demand of CaO all these influencing factors may be
incorporated in four parameters: SR, LS,
amount of oversized quartz grains,
amount of oversized calcite grains.
(Pressure, temperature and burning time
are considered to be constant.)
Silica ratio (SR) and lime saturation(LS)
The formation of C3S from C2S and CaO isgoverned by the diffusion of CaO through
the melt. The silica modules and lime
saturation are sufficient to describe this
chemical reaction quantitatively.
The amount of CaO which can beaccommodated within the liquid phase and
in which it can diffuse and thus react, is
inversely proportional to the silica ratio. Alinear relationship exists between max. lime
saturation and silica ratio values at which no
free lime can be observed.
Quartz and calcite grains Whether a grain of material reacts fully
under given burning conditions depends on
its diameter, structure and chemical
composition.
Too large calcite grains result in CaO notbeing completely combined as also results
from grains whose lime saturation is over
100 %.
-
7/27/2019 Clinker Formation Concepts
24/28
For the Holderbank burnability testconditions the following grain diameters
were found to be critical limits:
o quartz 32 mcalcite 90 m
====================================================
==========================
==========================
==========================================
Now to my linkedin colleges Ifinished the Fourth part of mylecture if you have any questioncontact me here or in my linkedin
account Or contact me by Email :
========================================================================
mailto:[email protected]:[email protected]:[email protected] -
7/27/2019 Clinker Formation Concepts
25/28
=============================================
Thermodynamics of Clinker Formation
During clinker production, heat is both absorbed (endothermic heat changes)
and produced (exothermic heat changes)
Temp. (C) Type of Reaction Heat Change
20 100 Evaporation of free H2 O Endothermic
100 300 Loss of physically adsorbed H2O Endothermic
400 900 Removal of structural H2O (H2O, OH groups from
clay minerals) Endothermic
600 900 Dissociation of CO2 from carbonate Endothermic
> 800 Formation of intermediate products, belite, aluminate and
ferrite Exothermic
> 1250 Formation of liquid phase (aluminate and ferrite
melt) EndothermicFormation of alite Exothermic
1300 1240 Crystallization of liquid phase into mainly (cooling cycle)
aluminate and ferrite Exothermic
Examples for exothermic reactions (heatliberated)
o Coal (C) + O2 CO2o Lime (CaO) + H2O Ca(OH)2o Cement + H2O Cement Hydrateso Liquid K2SO4 Solid K2SO4
Examples for endothermic reactions (heatabsorbed)
o H2O (liquid) H2O (steam)o CaCO3 CaO + CO2
=================================================
==================================================================================================
========
-
7/27/2019 Clinker Formation Concepts
26/28
DTA curves of typical cement raw meals
The greatest heat requirement occurs between 850 900 C, i.e. for the
decomposition of the carbonate minerals.The total heat requirements for
dehydration, decarbonisation and melting exceed the heat liberated by the
formation of belite and the intermediate and final products.
Endothermic processes kJ/kg clinker
-
7/27/2019 Clinker Formation Concepts
27/28
170dehydration of clays
1990decarbonisation of calcite
105heat of melting
2050heating of raw materials 0 1450 C
4315Total endothermic
Exothermic processes kJ/kg clinker
-40crystallization of dehydrated clay
-420heat of formation of clinker minerals
-105crystallization of melt
-1400cooling of clinker
-500cooling of CO2 (ex calcite)
-85cooling of H2O (ex clays)
-2550Total exothermic
Net theoretical heat of clinker formation + 1765
==============================================
==============================================
======================
Heat balance of wet and dry kiln, kJ/kg clinker
( HFW Taylor: Cement Chemistry, 1998 )
-
7/27/2019 Clinker Formation Concepts
28/28
Dry kiln Wet kiln
Evaporation of H2O 13 (0.4%) 2,364 (41.5%)
Heat of reaction 1,807 (54.6%) 1,741 (30.5%)
Heat losses through 711 (21.5%) 812 (12.3%)
gas, clinker, dust, etc.
Heat lost in air from cooler 427 (13.0%) 100 (1.7%)
Heat losses by radiation 348 (10.5%) 682 (12.0%)
and convection
3,306 kJ/kg 5,699 kJ/kg