differential dsc pt 1000 scanning …...5 the differential scanning calorimetry (dsc) is the most...
TRANSCRIPT
![Page 1: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/1.jpg)
DIFFERENTIAL SCANNING CALORIMETER
DSC PT 1000
T H E R M A L A N A L Y S I S
![Page 2: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/2.jpg)
2
Since 1957 LINSEIS Corporation has been deliv-
ering outstanding service, know how and lead-
ing innovative products in the field of thermal
analysis and thermo physical properties.
We are driven by innovation and customer sat-
isfaction.
Customer satisfaction, innovation, flexibility
and high quality are what LINSEIS represents.
Thanks to these fundamentals our company
enjoys an exceptional reputation among the
leading scientific and industrial organizations.
LINSEIS has been offering highly innovative
benchmark products for many years.
The LINSEIS business unit of thermal analysis
is involved in the complete range of thermo
analytical equipment for R&D as well as qual-
ity control. We support applications in sectors
such as polymers, chemical industry, inorganic
building materials and environmental analytics.
In addition, thermo physical properties of solids,
liquids and melts can be analyzed.
LINSEIS provides technological leadership. We
develop and manufacture thermo analytic and
thermo physical testing equipment to the high-
est standards and precision. Due to our innova-
tive drive and precision, we are a leading manu-
facturer of thermal Analysis equipment.
The development of thermo analytical testing
machines requires significant research and a
high degree of precision. LINSEIS Corp. invests
in this research to the benefit of our customers.
Claus Linseis Managing Director
![Page 3: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/3.jpg)
3
InnovationWe want to deliver the latest and best tech-
nology for our customers. LINSEIS continues
to innovate and enhance our existing thermal
analyzers. Our goal is constantly develop new
technologies to enable continued discovery in
Science.
German engineeringThe strive for the best due diligence and ac-
countability is part of our DNA. Our history is af-
fected by German engineering and strict quality
control.
![Page 4: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/4.jpg)
4
DIFFERENTIAL SCANNINGCALORIMETER
![Page 5: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/5.jpg)
5
The Differential Scanning Calorimetry (DSC) is
the most popular thermal analysis technique to
measure endothermic and exothermic transi-
tions as a function of temperature.
The instrument is used to characterize polymers,
pharmaceuticals, foods/biologicals, organic
chemicals and inorganics. Transitions measured
include Tg, melting, crystallization, curing, cure
kinetics, onset of oxidation and heat capacity.
Unsurpassed performance Revolutionary Sensor Design – Combined
Heat Flux & Power Compensation in one Sensor
Unsurpassed sensitivity – for detection of mel-
ts and weak transitions
Benchmark resolution – precise separation of
close lying events
Reliable Automation – up to 40 or 80 position
autosampler
Widest temperature range – from -180 °C to
725 °C in one measurement
The LINSEIS Differential Scanning Calorime-
ters (DSC) operates in agreement with natio-
nal and international standards such as: ASTM
C 351, D 3417, D 3418, D 3895, D 4565, E 793,
E 794, DIN 51004, 51007, 53765, 65467, DIN EN
728, ISO 10837, 11357, 11409.
LINSEIS DSC – 1000 MThis product was developed to provide a gene-
ral purpose DSC with a broad temperature range
(-150 up to 725°C) for all common applications.
Furthermore emphasis was placed on an extre-
mely stable baseline and high reproducibility.
The design allows manual and automatic ope-
ration. The conception of the cell guarantees
maximum mechanical and chemical resistance.
The high resolution metal sensor MHR provides
highest resolution and outstanding sensitivity.
UNSURPASSED SENSITIVITY
BENCHMARK RESOLUTION
UP TO 44/88 POSITION AUTO-SAMPLER
![Page 6: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/6.jpg)
6
![Page 7: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/7.jpg)
7
TECHNOLOGY
Reference Sample
Heater
Preheating for reaction gas
Metal sensor
LN2-Cooling
Intracooler
![Page 8: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/8.jpg)
8
SENSORSThe key part of every DSC is the sensor, so don’t
make any compromise. Up to now it has been
impossible to achieve highest resolution and
sensitivity in one sensor. The revolutionary de-
sign of the HiperRes® Sensor line now enables
just that. The high resolution MHR metal sensor
delivers outstanding resolution. This permits
the detection of smallest thermal effects. The
unique design ensures shortest possible time
constants, permitting the separation of overlap-
ping effects over the full temperature range.
MHRHigh resolution metal sensor ensures unparal-
leled resolution and durability. This sensor is
perfectly suited for day to day operation in re-
search and quality control.
SENSORS
Crucibles
![Page 9: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/9.jpg)
9
OPTIONS
Forced air cooling Quench air cooling system
One stage IntracoolerEnables controlled heating and cooling in the temperature range -40 up to 550°C.
Liquid Nitrogen QuenchingEnables controlled heating and uncontrolled cooling in the tem-perature range -150 up to 400°C. The accessory consists of a re-servoir which can be filled with Liquid Nitrogen, ice water, etc.
Liquid Nitrogen Cooling UnitEnables controlled heating and cooling in the temperature range -180 up to 750°C. This accessory consists of a Liquid Nitrogen De-war and an Electronic controlling the cooling speed.
Sample PressFor optimum sample preparation two different ergonomic sam-ple presses are available. One for pressure crucibles and one for standard crib and hermetic pans.
Intracooler Julabo FT900 DSC-Press
ACCESSORIES
![Page 10: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/10.jpg)
10
SOFTWAREAll LINSEIS thermo analytical instruments are
PC controlled. The individual software mod-
ules run exclusively under Microsoft® Windows®
operating systems. The complete software con-
sists of 3 modules: temperature control, data
acquisition and data evaluation. The Windows®
software incorporates all essential features
for measurement preparation, execution, and
evaluation of a thermoanalytical measurement.
Thanks to our specialists and application ex-
perts, LINSEIS was able to develop comprehen-
sive easy to understand user friendly applica-
tion driven software.
Features-Software:• Program capable of text editing
• Data security in case of power failure
• Thermocouple break protection
• Repetition measurements with minimum
parameter input
• Evaluation of current measurement
• Curve comparison up to 32 curves
• Storage and export of evaluations
• Export and import of data ASCII
• Data export to MS Excel
• Multi-methods analysis (DSC TG, TMA, DIL,
etc.)
• Zoom function
• 1 and 2 derivation
• Programmable gas control
• Curve arithmethics
• Statistical evaluation package
• Free scaling
• Optional Kinetic and Lifetime Prediction
Software packages
TG – Features:• Mass change as % and mg
• Rate Controlled Mass Loss (RCML)
• Evaluation of mass loss
• Residue mass evaluation
HDSC – Features:• Glass transition temperature
• Complex peak evaluation
• Multipoint calibration for sample temperature
• Multipoint calibration for change of enthalpy
• Cp calibration for heat flow
• Signal-steered measuring procedures
![Page 11: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/11.jpg)
11
Multi-Instrument All LINSEIS instruments DSC, DIL, STA, HFM, LFA,
etc. can be controlled from one software tem-
plate.
Report GeneratorConvenient template selection to generate cu-
stomized measurement reports.
Multi-Lingual Our software is available in many different
user exchangable languages, such as: English,
Spanish, French, German, Chinese, Korean,
Japanese, etc.
Multi-User The administrator can generate different user
levels providing different rights to operate the
instrument. A optional Log file is available, too.
Thermal Library
The LINSEIS Thermal Library software package
comes as an option for the well-known, user
friendly LINSEIS Platinum evaluation software
that is integrated in almost all our instruments.
Measured and matching reference curves (green) and reference curves with poor fit (red).
The Thermal Library allows you the comparison
of the complete curves with a data base provi-
ding thousands of references and standard ma-
terials within only 1-2 seconds.
Data BaseState of the art data base design enables easy
data handling.
Kinetic softwareKinetic analysis of DSC, DTA, TGA, EGA (TG-MS,
TG-FTIR) data for the study of the thermal beha-
vior of raw materials and products.
Material Identification
DSC curve recognition and
interpretation system
![Page 12: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/12.jpg)
12
![Page 13: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/13.jpg)
13
DSC PT 1000
Temperature range –150°C up to 725°C (low temperature with optional parts)
Heating and cooling rates 0.01 up to 100°C/min
Temperature accuracy +/- 0.2K
Temperature precision +/- 0. 2K
Digital resolution 16.8 million points
Resolution 0.03 μW
Atmospheres inert, oxidizing (static, dynamic)
Measuring range +/-2.5 up to +/-250mW
Calibration materials included
Calibration recommended 6 month interval
SPECIFICATIONS
![Page 14: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/14.jpg)
14
3.0
2.5
2.0
1.5
1.0
0.5
0
-0.5
-1.0
-1.5
-2.0
DSC
[mW
/mg]
500 600 700 800 900 1000 1100 1200 1300 1400 1500Temperature [°C]
exo
731.0°C
754.2°C
53.69J/g
1478.7°C
244.88J/g
1411.1°C1470.7°C
636.8°C
-240.22J/g
1436.4°C
1453.8°C
Heating
Cooling
Low Alloyed Steel
Temperature [°C]0 200 400 600 800 1000 1200 1400
Heat
Flo
w [m
W/m
G]
0.5
0.4
0.3
0.2
0.1
0.0
-0.1
-0.2
-0.3
h=-20.7 J/g
737°C
1031°C
1320°C
exo
DSC powder measurements of ferrites
The picture shows the specific heat flow rate of a low-alloyed steel sample, measured by HDSC. At 734°C the change in the crystal structure (from body center to face center) and the change in the magnetic proper-ties (ferromagnetic to parama-gnetic) occurred. The melting point can be seen at 1411°C. The liquidus temperature was measured at 1473°C. All peaks are reversible and can be ob-served in the cooling segment as well. The phase transition to ferromagnetic takes place at 637°C and the crystallization range goes from 1454°C to 1436°C.
Food
The components used for pro-duction of magnetic ferrites are ZnO, Fe2O3 and Cr2O3. The Chrome oxide is added for modification of magnetic and electric properties.At 735°C the powder forms a mixed ferrite with a spinal struc-ture (exothermal reaction: -20.6 J/g).Above 1034°C and 1321°C the heat flow changes into the endothermic direction due to melting of different phases.The LINSEIS DSC PT1600 with type S measuring sensor pro-vides a very stable baseline with an extremely low noise level up to 1600°C. This high sensitivity is essential to perform exact re-action enthalpy measurements and evaluations.
APPLICATIONS
![Page 15: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/15.jpg)
15
0
-10
-20
-30
-40
-50
Mas
s Ch
ange
[%]
0 200 400 600 800 1000
2
1
0
-1
-2
-3
-4
d(TG
)/dt
[%/m
in]
80
60
40
20
0
-10
DTA
[µV
(exo
)
]
d(TG)
DTA
598.2°C
773.3°C845.2°C
921.7°C
477.8°C608.2°C
787.0°C848.3°C
939.5°C
Temperature [°C]
Talcum (Mg3(OH)2[Si2O5]2) is a mineral that consists of hydra-ted magnesium silicate. It is used for the production of ste-atite bodies used as isolators with high resistance and a low dielectric loss factor. Its impu-rities (chlorite, carbonates) can be determined and detected using DSC.The measurement shows the dehydroxylation of chlorite that appears at 608°C and 848°C as endothermal DSC signals. At 768°C the removal of CO2 can be observed when the con-tained carbonates decompose into their oxides, releasing the CO2. Finally the dehydroxylati-on of talc can be seen at 937°C as an endothermal peak as well.
Modulated Cp determination
HD
SC [µ
V]
Time [min]0 10 20 30 40 50 60 70 80 90 100 110 120
5.0
0
-5.0
-10.0
800
700
600
500
400
300
200
1.70
1.60
1.50
1.40
1.30
1.20
1.10
1.00
0.90
0.80
0.70
Cp mod Saph raw data (HDSC)
Tem
per
atu
re [°
C]
Cp
[J/(
gK
)]
Cp mod Saph (Cp|a)
Saph Lit. value (Cp)
For highest possible accuracy of Cp, the LINSEIS DSC allows the usage of modulated heating rate temperature profiles. This method causes a continuous change in heat flow of the sam-ple and the system can monitor the heat uptake much better than with a linear heating pro-file. The deviation from the li-terature value is much smaller than with linear DSC runs.The modulated heat flow signal (black) leads to a significant better Cp resolution (dark blue) that is only slightly different from the literature (bright blue) over the full temperature range. The orange curve shows the modulated heating profile.
DSC Analysis of Talcum
![Page 16: DIFFERENTIAL DSC PT 1000 SCANNING …...5 The Differential Scanning Calorimetry (DSC) is the most popular thermal analysis technique to measure endothermic and exothermic transi-tions](https://reader035.vdocument.in/reader035/viewer/2022062506/5f0d78987e708231d43a8538/html5/thumbnails/16.jpg)
LINSEIS GmbH Germany
Vielitzerstr. 43
95100 Selb
Tel.: (+49) 9287–880 - 0
Fax: (+49) 9287–70488
E-mail: [email protected]
LINSEIS China
Kaige Scientific Park 2653 Hunan Road
201315 Shanghai
Tel.: (+21) 5055 0642
Fax.: (+21) 6806 3576
LINSEIS Poland
Dabrowskiego 1
05-800 Pruszków
Tel.: (+48) 692-773-795
LINSEIS Inc. USA
109 North Gold Drive
Robbinsville, NJ 08691
Tel.: (+1) 609 223 2070
Fax: (+1) 609 223 2074
E-mail: [email protected]
LINSEIS France
Bureaux Paris
52 Boulevard Sébastopol
75003 Paris
Tel.: (+33) 1 73.02.82.72
www.linseis.com
Products: DIL, TG, STA, DSC, HDSC, DTA, TMA, MS/FTIR, In-Situ EGA, Laser Flash, Seebeck Effect, Thin Film Analyzer, Hall-Effect
Services: Service Lab, Calibration Service
08/17