STRESS-CORROSION FATIGUE CRACKING
OF COLD EXPANDED COMPONENTS
by
RAMKUMAR KUNNAVAKKAMVINJAMUR, B.E.
A THESIS
IN
MECHANICAL ENGINEERING
Submitted to the Graduate Faculty of Texas Tech University in
Partial Fulfillment of the Requirements for
the Degree of
MASTER OF SCIENCE
IN
MECHANICAL ENGINEERING
Approved
May, 2002
ACKNOWLEDGMENTS
I would like to thank my graduate advisor, Dr. Jahangir Rasty for his support and
guidance throughout my graduate studies and research. I would also like to express my
sincere gratitude to Dr. Atila Ertas and Dr. Stephen Ekwaro-Osire for serving on my
thesis committee.
I would like to thank Dr. Mark Grimson and Dr. Candace Haigler of Electron
Microscopy Laboratory for their assistance while generating the photographs of fracture
surfaces. 1 am also very grateful to Dr. Thomas Burton and Department of Mechanical
Engineering, Texas Tech University for giving me the opportunity to pursue my graduate
studies.
I would also like to acknowledge with thanks helps rendered by Dr. Xiaobin Le,
Mr. Ron Bermett and Mr. Kevin Kerr during testing. I also highly appreciate the help
rendered by Mr. Norman Jackson and machine shop staff during the machining of the
specimens.
Finally, I would like to thank my parents and friends for their support and
encouragement during my academic career.
TABLE OF CONTENTS
ACKNOWLEDGMENTS ii
ABSTRACT vi
LIST OF TABLES viii
LIST OF FIGURES ix
GLOSSARY xi
CHAPTER
I. INTRODUCTION 1
1.1 Background 1
1.1.1 Cold Expansion Technology 1
1.1.2 Sfress Corrosion Fatigue Cracking 2
1.2 Literature Review 4
1.3 Objectives 7
II. EXPERIMENTAL PROCEDURE 8
2.1 Corrosion of Specimens 8
2.1.1 Masking of the Sample 8
2.1.2 Corrosion Cell 9
2.1.3 Corrosion Rate Determination 12
2.1.4 Corrosion of the Samples 12
2.1.5 Cleaning and weighing of Samples 14
2.2 Fatigue Testing of the Specimens 15
111
2.2.1 S ystem Parameters 15
2.2.2 Trial Runs 15
2.2.3 Sample Preparation for Fatigue Testing 17
2.2.4 Testing 21
2,3 Fractographic Analysis 21
2.3.1 Specimen Preparation 21
2.3.2 Analysis 24
III RESULTS AND DISCUSSIONS 28
3.1 Mass Loss Results 28
3.2 Tensile Test Results 32
3.3 Fatigue Test Resuhs 32
3.4 Statistical Analysis 38
3.4.1 ANOVA for 3 - factorial design 41
3.4.2 ANOVA for 3 ' x 2' factorial design 47
3.5 Fractographic Analysis Results 53
3.5.1 (0,0) Specimen 53
3.5.2 (0,10) Specimen 56
3.5.3 (2,10) Specimen 56
3.5.4 (2,20) Specimen 59
3.5.5 (4,20) Specimen 60
rv CONCLUSIONS AND RECOMMENDATIONS 67
4.1 Conclusions 67
4.2 Recommendations ^o
REFERENCES ^^
ABSTRACT
Fasteners like rivets are widely used for assembling parts in the aircraft industry.
The fasteners not only help in easy assembly and dismantling of the parts, but also help in
proper distribution of the load applied on the body. However, in order to fasten two parts
together, a number of holes have to be drilled on both parts and these holes tend to raise
the sfress in the region surrounding them. This sfress concenfration effect of the holes
reduces the fatigue life of the part when cyclic load is applied to the part. To offset the
sfress concenfration effect of the holes, a technique called Split Sleeve Cold Expansion
has been widely used in the aircraft industry. It induces a compressive residual sfress in
the fastener hole and the region aroimd it, which retards the growth of fatigue crack and
thereby improves the fatigue life of the component.
The objective of this thesis work was to analyze the effect of Split Sleeve Cold
Expansion on the fatigue life of AI-7075 T6 specimen subjected to corrosion. In order to
fiilly understand the interaction between cold expansion, corrosion and fatigue life, two
possible cases were considered. In the first case the specimens were cold expanded first
and then corroded to required mass loss level. In the second case the specimen were
corroded prior to cold expansion. The specimens were corroded using a galvanic
corrosion cell. The specimens were then tested for fatigue sfrength.
The results showed that cold expansion improved the fatigue life of xm-corroded
and mildly corroded specimen by a factor of 20. However, fatigue life of cold expanded
specimens dropped exponentially with corrosion. For severely corroded specimens there
vi
was no significant improvement in fatigue life due to cold expansion. The results also
showed that for specimens subjected to the same degrees of cold expansion and
corrosion, the fatigue life of specimens cold expanded after corrosion was lower than the
fatigue life of specimens cold expanded prior to corrosion.
Vll
LIST OF TABLES
2.1 Order of test runs for full factorial 3 ^ x 2 ' experiment 22
2.2 Description of codes used in Table 2.1 23
3.1 Mass Loss (ML), in grams, for various corrosion exposure times (hours) 29
3.2 Tensile Test Data for A1-7075-T6 32
3.3 Fatigue test data for cold expanded specimens subjected to subsequent corrosion 34
3.4 Fatigue test data for corroded specimens subjected to subsequent cold expansion 36
3.5 Fatigue life data for balanced 3 ^ factorial design 42
3.6 ANOVA for balanced 3 ^ factorial design 43
3.7 Fatigue life data for unbalanced 3 ^ factorial design 44
3.8 ANOVA for unbalanced 3^ factorial design (Type I) 45
3.9 ANOVA for unbalanced 3 ^ factorial design (Type III) 46
3.10 Fatigue hfe data for balanced 3 ^ x 2 ' factorial design 48
3.11 ANOVA for balanced 3 ^ x 2 ' factorial design 49
3.12 Fatigue hfe data for unbalanced 3" x 2' factorial design 50
3.13 ANOVA for unbalanced 3 ' x 2' factorial design (Type I) 51
3.14 ANOVA for unbalanced 3 ' x 2' factorial design (Type III) 52
VlU
LIST OF FIGURES
1.1 Split Sleeve Cold Expansion 3
2.1 Masked specimen prior to corrosion 10
2.2 Corrosion cell 11
2.3 Corroded specimen prior to fatigue tests 13
2.4 Insfron testing machine used for fatigue testings 16
2.5 Schematic of fatigue test specimens 18
2.6 Split Sleeve cold expansion tool 20
2.7 Sputter coater 25
2.8 Scarming Elecfron Microscope 27
3.1 Corrosion mass loss versus Time 31
3.2 Fatigue life of cold expanded specimens subjected to subsequent corrosion 35
3.3 Fatigue of corroded specimens subjected to subsequent cold expansion 37
3.4 Comparison of fatigue hfe of specimens cold expanded prior to corrosion and specimens cold expanded after corrosion at CET=2 % 39
3.5 Comparison of fatigue life of specimens cold expanded prior to corrosion
with specimens cold expanded after corrosion at CET = 4 % 40
3.6 Appearance of edge of (0,0) specimen 54
3.7 Appearance of surface along the length of (0,0) specimen 55
3.8 Fatigue striations for (0,0) specimen 57
3.9 Appearance of the edge of (0,10) specimen 5 8
IX
3.10 Corroded edge for (2,10) specimen 61
3.11 Appearance of fracture surface for (2,10) specimen 62
3.12 Appearance of fracture surface for (2,10) specimen on the other side 62
of the hole
3.13 Corroded edge for (2,20) specimen 63
3.14 Corroded edge for (4,20) specimen 64
3.15 Surface on the left side of the hole for (4,20) specimen 65
3.16 Appearance of the surface on the right side of the hole for (4,20) specimen 66
GLOSSARY
(0,0) Unfreated specimens.
(2,0) Un-corroded specimens subjected to 2% cold expansion.
(4,0) Un-corroded specimens subjected to 4% cold expansion.
(0,10) Non-cold expanded specimens subjected to 10% mass loss due to corrosion.
(0,20) Non-cold expanded specimens subjected to 20% mass loss due to corrosion.
(2,10) Specimens subjected to 2% cold expansion and 10% mass loss due to corrosion.
(2,20) Specimens subjected to 2% cold expansion and 20% mass loss due to corrosion.
(4,10) Specimens subjected to 4% cold expansion and 10% mass loss due to corrosion.
(4,20) Specimens subjected to 4% cold expansion and 20% mass loss due to corrosion.
XI
CHAPTER I
INTRODUCTION
1.1 Background
1.1.1 Cold Expansion Technology
Fasteners like rivets and bolts are widely used for assembling parts in the afrcraft
industry, where a number of parts are riveted together to form aircraft structures. Not
only do these fastened joints enable easy assembly and dismantUng, they are also able to
transfer as well as distribute loads applied onto the structure. However, in order to rivet
the parts to build the structure, a number of holes have to be drilled in the parts. These
holes are a significant source of stress concentration, and in the presence of cyclic tensile
stress, they act as primary sources of fatigue cracks that originate from microscopic
defects in the material. Over a period of time, these cracks begin to grow and result in
fatigue failure of the structure.
Many systems have been conceived to offset this stress concentration effect of
fastener holes. The underlying principle of all these systems is to induce permanent
compressive stress near the hole, which could prevent fatigue cracks that originate from
the edge of the holes. One such system, which has been widely used in the aircraft
industry, is the Split Sleeve Cold Expansion process. This process was conceived by the
Boeing Company and later developed as an integrated system by Fatigue Technology Inc.
(Rufin, 1993 ). This process uses a tapered mandrel in conjunction with a disposable, pre-
lubricated spUt sleeve to compressively pre-sfress a significant zone around the fastener
hole. The compressive stresses are generated by pulUng the tapered mandrel, pre-fitted
with the sleeve, through the hole. The mandrel and the sleeve radially expand the hole
creating an annular zone of compressive stress around the hole. This pre-stressing offsets
the stress concentiration of the hole to produce substantial improvements in the fatigue
performance of the fastened joints. The compressive zone also arrests the growth of pre
existing cracks in the material. Figure 1.1 shows the process.
1.1.2 Stress Corrosion Fatigue Cracking
Stress corrosion fatigue cracking is essentially fatigue fracture aggravated by the
effects of the envfroimient. American Society for Metals defines it, as "Effect of the
appUcation of repeated or fluctuating stresses in a corrosive envfronment characterized by
shorter life than would be encountered as a result of either the repeated or fluctuating
stresses or corrosive envfronment" (Corrosion, vol 13, ASM Handbook, 1987).
The fatigue hfe of the part is strongly affected by the type of cycUc stressing. The
longer and more frequentiy a fatigue crack is opened, the more will be the effect of
envfronment on shortening the fatigue hfe. In many cases the fatigue crack is initiated
from smaU pits on the corroded surface, which act as stress concentration points. In other
cases the fatigue crack initiates ffrst and is then made to grow more rapidly by moisture
or other corrodents that enter the crack by capillary action.
This type of cracking is most frequentiy encountered in ships, afrcrafts and
structures that are frequently exposed to corrosive envfronments and fluctuating loads
and is a major problem as the fatigue Ufe is reduced cfrasticaUy.
^- Nosrcap Mandfet
/
Split Sleevp
(a)
Ai-«-a ^ r C r f l d K,5>panis,iois
S Z Z S Z ^ ^ ^ ^ ^ & ^
(b)
Figure 1.1: SpUt sleeve cold expansion, (a) Parts of the Split Sleeve Cold Expansion tool, (b) Shows the cold expansion process (Rufin, 1993).
1.2 Literature Review
A large volume of hterature is available on cold expansion due to its widespread
use in the afrcraft industry. The research work dates back to the 1970s when the Split
Sleeve Cold Expansion system was developed by the Manufacturing Research and
Development Organization of Boeing Commercial Airplane Company. PhiUips (1973) of
Boeing Commercial Airplane Company provided an overview of the process and
summarized the results that were obtained from Afr Force Materials Laboratory (AFML)
sponsored tests on aerospace materials. The results showed that compressive residual
stresses induced during the cold expansion process effectively arrests crack growth from
the hole and significantiy improves fatigue Ufe of the specimen.
Petrak and Stewart (1976) did some of the earUest work on cold expansion. They
carried out tests to evaluate the capabiUty of cold expansion and other interference
fastener systems to retard crack growth from fastener holes. They tested Al-7075 T6
alloys with pre-existing cracks in the holes and showed that the cold expansion and
interference fastener systems effectively retarded crack growth.
Later, Chandawanich and Shaipe (1979) studied the effect of cold expansion on
crack initiation and crack growth rate in Al-7075 T6 alloys. They showed that while cold
expansion did not affect the crack initiation, it retarded the crack propagation rate and
thereby increased the fatigue hfe of the specimen. More recentiy, Rachid et al. (2000)
demonstrated that Split Sleeve Cold Expansion affects the crack nucleation stage by
causing changes in the microstructure of the material near the surface. Rufin (1993)
presented a paper describing the effectiveness of SpUt Sleeve Cold Expansion in
improving the fatigue Ufe of an engine. The papers also showcased the abiUty of SpUt
Sleeve Cold Expansion to arrest fatigue cracks in holes with low edge/margin ratio. He
also showed that cold expansion could be used effectively for components working at
high temperatures.
Even though SpUt Sleeve Cold Expansion was initially intended for new
production afrcraft structures, the process has been effectively used for in-service repairs.
Reid (1997) described how cold expansion could be used to enhance the integrity and
durabiUty of repafrs. Gaerke et al. (2000) stucUed the benefits of cold expanding fastener
holes at various stages of fatigue Ufe in AI-2024 T 31 low-load transfer joint. The authors
pre-cycled the specimen to 25%, 50%, 75% baseUne fatigue Ufe of the non-expanded
specimen and then cold expanded the components prior to final cycUng to failure. The
tests showed that part-Ufe cold expansion could provide substantial improvements in
fatigue Ufe.
A number of analytical and finite element methods for predicting the residual
stresses induced by cold expansion have been developed over a period of years due to the
importance of knowing the residual stress field around the hole to predict the crack
growth rate. Ozdemfr and Edwards (1996) developed a method to predict the residual
stress distribution around the hole through the use of Sachs method. They also showed
that the orientation of the spUt on the expansion sleeve affects the distribution of residual
stresses. Dutta (1997) developed a finite element model to identify the process variables
confrolUng the effectiveness of the cold expansion technology. The author along with
Rasty (1999) also developed analytical equations for determination of the elastic-plastic
boundary radius, using a far field strain measurement. The elastic-plastic boundary was
then used for determining the residual stress distribution.
The effect of corrosion on fatigue Ufe of components is widely researched due to
its detifrnental impact on the fatigue Ufe of the component. Sankaran et aL (2001) showed
tiiat pitting corrosion in Al-7075 T6 components can reduce the fatigue Ufe of the
component by 6-8 times. Chen et al. (1996) showed that failure in corroded specimens
occur due to fatigue cracks nucleating from pits formed on the surface due to corrosion.
When the region close to the hole is corroded, then the combined stress concentration
effects of the hole and the rough surface produced by corrosion can severely reduce the
fatigue Ufe of the component. Moesser et aL (1995) studied the effect of corrosion near
die fastener hole on fatigue Ufe of the component.
Due to the serious problems posed by the interaction between corrosion and
fastener hole, the effect of cold expansion in retarcUng stress corrosion fatigue crack
propagation has been researched. Cook et al. (1996) studied the effect of pitting corrosion
on cold expanded holes. They also stucUed the interaction between the tensile residual
stresses induced by cold expansion away from the hole and stress corrosion cracking.
They also demonstrated that when a specimen is cold expanded after corrosion, the
fatigue life of the specimen is lower than when the specimen is cold expanded prior to
corrosion.
fri this thesis work, the effect of cold expansion on stress corrosion fatigue
cracking is studied. UnUke the other works, the extent of corrosion here is quantified by
using mass loss as measuring parameter.
1.3 Objectives
The three objectives of this research were: (1) To study the effect of corrosion on
fatigue Ufe of non-treated Al 7075-T6 specimens, (2) to study the effect of cold
expansion on fatigue Ufe of specimens corroded after cold expansion, (3) to study the
effect of cold expansion on fatigue Ufe of specimens corroded prior to cold expansion.
CHAPTER n
EXPERIMENTAL PROCEDURE
2.1 Corrosion of Specimens
2.1.1 Masking of the Sample
This experiment requfred only a smaU region of the specimen around the hole to
be corroded in order to study the interaction between corrosion and cold expansion.
Therefore, it was necessary to protect the remaining regions from corrosion using a
corrosion-inhibiting mask. 3-M AU-Weather Corrosion Protection Tape was used for tiiis
purpose. The tape was appUed on the regions of the sample that were to be protected
from corrosion. Some cUfficulty was encountered in finding a suitable method for
applying the tape.
Initially, the tape was appUed in an overlapping maimer over the sample, leaving
a smaU rectangular region in the middle of the sample exposed. This was found to yield
poor results due to leakage along the overlapping edges. Also, the tape tended to peel off
over prolonged periods of exposure, resulting in corrosion of masked areas of the
specimen.
In order to correct this problem, rectangular strips corresponding to the areas to be
exposed were cut out from the tape before applying it to the specimen. The areas to be
exposed were carefully marked on the front and the backside of the sample. The mask
was then appUed over the sample by carefuUy aUgning the tape and the sample. This
method was found to yield good results for the corrosion rates used in this experiment.
There was no leakage around the mask and the corrosion was restricted to the exposed
region.
However, for very severe corrosion (close to 35 % removal of material by weight)
this method was found to be inadequate. There was leakage around the mask due to
difference in the thickness between the corroded and masked regions. Due to this, some
portions of the masked region were also corroded. But, for the corrosion levels used in
this experiment the masking was found to yield good results. An example of the masked
specimen can be seen in Figure 2.1.
2.1.2 Corrosion CeU
Accelerated corrosion of the samples was carried out using a galvanic corrosion
ceU. The ceU consisted of an 8-gaUon plastic container, electrolyte, anode, catiiode and a
power source. The masked aluminum sample was used as anode and was coimected to
the positive terminal of the constant current power source. Two Al-7075 T6 plates were
used as cathodes to corrode both sides of the specimen. The cathodes were connected to
the negative terminal of the power source. The electrolyte used was a 2% salt solution
prepared by dissolving aquarium salt in distiUed water. The Ph of the electirolyte was
maintained at around 8 and the temperature was maintained at 70 degrees Fahrenheit.
The anode and tiie catiiodes were immersed in the electrolyte and a constant current of 50
mA / in^ was appUed across the electi-odes. Figure 2.2 shows the ceU used for corroding
the specimen.
''//^V';i;^ "p^^'^rf'^f^.
Figure 2.1: Masked specimen prior to corrosion.
10
(a)
(b)
Figure 2.2: Corrosion ceU (a) front view and (b) top view
11
2.1.3 Corrosion Rate Determination
In order to determine the time taken to corrode the sample to requfred mass loss
levels, several trial samples were corroded. The trial samples were 1.6 inches in width
and 5 inches in length. The samples were typicaUy 0.1 inch in thickness. The samples
were masked and corroded for a period of 30 hours and the mass loss was noted at 1-hour
intervals. The recorded data were then used to fit a curve to predict the time requfred to
corrode the sample to requfred mass loss level. This model was tested for accuracy and
found to yield good results.
2.1.4 Corrosion of the Samples
The samples to be tested were corroded one at a time in the corrosion ceU. They
were immersed in the electrolyte and a constant current density of 50 mA / in^ was
maintained across the electrodes. The samples were removed at the end of time requfred
to reach the desfred mass loss level.
As a result of the corrosion, there was a buildup of corrosion products on the
surface of the cathodes. This material was removed periodically using a wfre brush. The
temperature and Ph of the electrolyte were carefuUy monitored and the electrol5l;e was
changed if there were any deviations. The electrolyte was also changed regularly at 10-
hour intervals to remove the corrosion products. Figure 2.3 shows a corroded sample
12
••i-^ ' A ;
•i -*• ' • i - * '" ! '
I * • — • • .
Figure 2.3: Corroded specimen prior to fatigue testing.
13
2.1.5 Cleaning and Weighing of Samples
After removing the samples from the corrosion cell, the samples were unmasked
and cleaned. The corrosion products on the surface of the sample were gentiy removed
using a plastic brush. The samples were further cleaned using 30% nitric acid solution
according to ASTM Gl standard. The samples were then washed in distiUed water and
dried using a hafr dryer.
The samples were then weighed using a Sartorius Analytic scale, model A210P,
with precision of 1/10000 of a gram. The weight of the sample before and after corrosion
was recorded and was used to calculate the percentage mass loss using the formula.
Percentage mass loss = Am /(L * W * T * p) (2.1)
Where Am = weight of material removed by corrosion
L = length of corroded region
W = width of the corroded region
T = thickness of the corroded region
p = density of Al-7075 T6 aUoy.
The mass loss percentage was recorded and tiie samples were marked for identification.
14
2.2 Fatigue Testing of the Specimens
2.2.1 System Parameters
Fatigue testing of the samples was done using a servo hydrauUc testing machine.
The machine consisted of an MTS load frame (MiimeapoUs, MN) with Instron grips and
hydrauUcs (Canton, MA). The testing system was controUed using a desktop PC.
Wavemaker-Runtime (Version 5.1), developed by Inston was used for signal control and
data acquisition. Figure 2.4 shows the system used for fatigue testing.
The fatigue tests were conducted at 10 HZ frequencies with the load varying from
2500 Ibf to 250 Ibf. The maximum and minimum loads to which the samples were to be
subjected were calculated using the modified-Goodman equation.
Wavemaker software was used for generating the program to control the fatigue
test. To get the requfred load cycles, a ramp function of magnitude 1375 Ibf was appUed
followed by a sine function with ampUtude varying from -1-1125 Ibf to -1125 Ibf. This
resulted in the desfred range of 250 Ibf to 2500 Ibf.
2.2.2 Trial Runs
The samples used for trial runs were typicaUy 12 inches in length and 1.6 inches
in width with a thickness of 0.1 inch. A hole of diameter 0.219 inches was driUed in die
samples. Trial runs were performed to determine the area of the specimen to be corroded
so that it fractures across the hole. This was requfred in order to study the effect of cold
expansion.
15
Figure 2.4: Instron testing machine used for fatigue tests
16
Initially, a region of lengtii 2.5 inches and widdi 1.6 inches was corroded to 5%,
10%, 15% and 20% mass loss and tested. The non-cold expanded specimen fractured
across the hole, but when the specimen was cold expanded to 2% or 4% the results were
unpredictable. The specimen fractured away from die hole along the bottom edge of the
corroded region and it was not possible to analyze the effect of cold expansion.
Therefore, the area to be corroded was reduced to a smaU rectangular strip of
length 0.219 inches and width 1.6 inches. This yielded good resuhs for non-cold
expanded samples. When the samples were cold expanded and tested, it was found that
some of the samples fractured due to cracks originating from outer edges.
To ensure that the cracks originate from the hole the edges of the specimen were
masked and the exposed area was reduced to a rectangular strip 0.219 inches in length
and 1 inch in width. This sample fractured consistentiy through the holes from cracks
originating from the holes.
2.2.3 Sample Preparation for Fatigue Testing
The samples to be used for actual testing were cut out from Al-7075 T6 aUoy
sheets into rectangular strips of length 12 inches and width 3 inches along the dfrection of
roUing. These rectangular strips were machined to dog bone shape using HAAS VF-3
Computer Numerical Control MiU (HASS Automation, Inc. L.A., CA). Figure 2.5 shows
the dimension of the specimen. The gage area of the sample was 2.5 inches in length and
1.6 inches in width. A hole of diameter 0.219 inches was driUed in the sample. A total
of 60 samples were machined using the CNC miU.
17
3,00
Figure 2.5: Schematic of fatigue test specimens. (All dimensions are in inches)
18
The machined samples were divided into two groups. The first set of samples
was prepared by cold expanding the samples to 0%, 2%, 4 % and then corroding
them to 0%, 10% and 20% mass loss. The second set was prepared by corroding the
samples fu"st prior to cold expansion.
The samples were cold expanded using the SpUt Sleeve Cold Expansion (SsCx)
System developed by Fatigue Technology Inc., CA. SpUt sleeves of thickness 0.0080
inches (# 2116-312) were used in combination with mandrel of nose diameter 0.2119
inches (# 2025-174) for 4% cold expansion. For 2% cold expansion, the same sleeve was
used with a mandrel of nose diameter 0.2070 inches (# CBM-6-2-N-1-30-V2). Figure 2.6
shows the system used for cold expansion. The percentage cold expansion was
calculated using the formula.
D +2W-Z), ,^^^ Percentage expansion = — (2.2)
Where D = Nose diameter of the mandrel
D;, = Diameter of the hole
W = Sleeve thickness.
The samples were corroded to three mass loss levels, namely 0%, 10% and 20% mass
loss, using the galvanic ceU described previously. Mass loss levels were determined from
trial runs based on number of cycles requfred to fracture the specimen. The samples were
corroded in the galvanic cell by applying a constant current density of 50 mA/in.sq across
the electrodes.
19
~.''-->^
Figure 2.6: SpUt Sleeve cold expansion tool
20
2.2.4 Testing
The fatigue testing of the samples was carried out using the system described
previously. The order in which the samples were to be tested in the machine was
completely randomized using random number tables. This was done in order to reduce
the effect of extraneous factors that might affect the machine. Table 2.1 shows the order
in which the samples were tested. Table 2.2 shows the coding used in Table 2.1. The
samples were run to a maximum of 2 milUon cycles. The tests were stopped at this point
if the samples did not break due to time constraints.
2.3 Fractographic Analysis
2.3.1 Specimen Preparation
Fractured samples from the fatigue tests were used for conducting fractographic
analysis. Fracture surfaces from the fatigue test samples were machined and mounted on
aluminum pedestals using STR tapes. The specimens were then grounded to the pedestal
using coUoidal silver paste. TypicaUy die specimens used for analysis were 1.6 inches in
width and 0.3 inches in height.
When observed under die microscope, the specimen tends to expand or even melt
due to the heat generated by the electrons bombarding the surface. In order to prevent
over-heating of the surface the specimen has to be sputter coated.
Sputter coating in tiiis case was done using Techics Hununer V Sputter Coater.
This coater uses argon gas as inert gas and plates eitiier gold or gold/paUadium on
21
Table 2.1: Order of test runs for full factorial 3^ x2 ' experiment
Test run
1
2
3
4
5
6
7
8
9
10
11
12
13
14
15
16
17
18
19
20
21
22
23
Cold expansion
0
1
-1
1
0
0
0
-1
0
0
1
-1
1
0
1
0
0
0
0
1
0
1
1
Corrosion
0
1
1
0
0
1
0
-1
1
1
0
-1
0
-1
1
0
-1
1
0
1
-1
1
-1
Order
1
1
1
1
2
1
1
1
2
1
2
1
1
1
2
2
1
1
2
1
1
2
1
22
Table 2.1.Continued
Test run
24
25
26
27
28
29
30
31
32
33
34
35
36
37
38
39
Cold expansion
1
-1
-1
1
1
0
-1
0
-1
1
1
-1
1
1
-1
0
Corrosion
1
1
-1
0
0
0
• 0
1
1
1
-1
0
0
-1
0
1
Order
1
1
1
2
2
1
1
2
1
2
1
1
1
1
1
2
Table 2.2: Description of Codes used in Table 2.1
Cold expansion (%)
0
2
4
Code
-1
0
1
Corrosion (%)
0
10
20
Code
-1
0
1
Order
Cold expanded first
Corroded first
Code
1
2
23
die specimen. The plating was done in a vacuum chamber, which was maintained at a
vacuum pressure of around 50-70 mTorr. During die process the voltage across the
electrodes in die vacuum chamber was set at 10 Volts and the current was maintained at
10 mA by varying die pressure control dial. The diickness of die plating given by die
sputter coater was controlled by setting die time on die process conti-ol timer. In diis case
die timer was set at 2 minutes to give 200 Angsti-om diick plating on die specimen.
Figure 2.7 shows die sputter coater used for preparing die specimen. Ten specmiens, two
each for (0,0), (0,10), (2,10), (2,20) and (4,20) cases were prepared usmg die sputter
coater.
2.3.2 Analysis
Fractographic analysis was done using a Hitachi S-570 Scanning Electron
Microscope. The specimen to be analyzed was mounted onto a pedestal in the column of
the microscope. This column was typicaUy maintained at a vacuum pressure of 0.0001
Torr in order to aUow passage of electrons without interference.
The Hitachi S-570 uses a tungsten filament, 0.1 nm in diameter, to generate the
electrons. The emission rate from the filament was controUed by varying the filament
current using the filament pot. The filament pot was adjusted to saturate the filament
properly to get a good image. The elecfrons generated by the filament were then
accelerated towards the specimen by applying an accelerating voltage. The accelerating
voltage was typicaUy set at 12 KV.
24
i"
en . » • • ' • ' • • ' ,» » ./ 4*
O:
Figure 2.7: Sputter coater (Techics Hummer v sputter coater)
25
The S-570 uses two electromagnetic lenses to properly focus the electron beam
generated by the filament properly on the specimen's requfred spot. It is important to
aUgn the filament and the lenses to get a good image. This aUgnment was done using
beam aUgnment controls, which centers the filament properly with respect to the
condenser lens. Further, the stigmator associated with the objective lens was also adjusted
using stigmation controls in order to remove astigmatism errors in the electron beam.
The image generated on the screen was then focused using coarse and fine focus
contirols. Further, die working distance, aperture opening, condenser lens current and tilt
angle were also varied in order to get good resolution and depth of focus in the image.
The final image generated on the screen was then captured using a Kodak camera
mounted on the microscope. Figure 2.8 shows a picture of the scanning electron
microscope used.
26
Figure 2.8: Scanning Electron Microscope (Hitachi S-570)
27
CHAPTER ni
RESULTS AND DISCUSSIONS
3.1 Mass Loss Results
The mass loss data for the trial samples were recorded every hour for 30 hours.
Table 3.1 shows the total mass lost by the trail samples and the time taken for it. The data
from this table were used to fit a curve given by the equation 0.00002972 x ̂ -i- 0.00579 x
- 0.0009, which predicts the mass loss as a function of time. A plot of the curve and the
data used to fit the curves is shovra in Figure 3.1. The plot shows that the values
predicted by the fitted curve differ from the actual values ± 10% especiaUy at around 20
hours and above. In order to compensate for this difference between the predicted values
and the actual values the test specimens were weighed three hours before the predicted
time and depending on the mass loss they were further corroded. By this method, it was
possible to corrode the test specimen to within ± 1 % of requfred mass loss.
28
Table 3.1: Mass loss (ML), in grams, for various corrosion exposure times (hours)
Time (hours)
1
2
3
4
5
6
7
8
9
10
11
12
13
14
15
16
17
18
19
M L -Run 1
0.0048
0.010
0.0167
0.023
0.0293
0.0353
0.0422
0.0488
0.0544
0.062
0.0686
0.0753
0.082
0.0888
0.0954
0.1024
0.1094
0.1164
0.1233
M L - Run 2
0.0048
0.0108
0.016
0.0231
0.0293
0.0356
0.0412
0.0475
0.0535
0.0594
0.0653
0.0713
0.0771
0.0831
0.0893
0.0956
0.1019
0.1082
0.1145
M L -Run 3
0.0048
0.0104
0.0164
0.0223
0.0282
0.0341
0.0404
0.0466
0.0529
0.0595
0.0661
0.0727
0.0793
0.0859
0.0929
0.0998
0.1068
0.1138
0.1215
Average M L
0.0048
0.0103
0.0164
0.0228
0.0289
0.0350
0.0412
0.0476
0.0539
0.0603
0.0667
0.0731
0.0794
0.0858
0.0925
0.0992
0.1060
0.1128
0.1197
M L from fitted curve
0.0049
0.0108
0.0167
0.0227
0.0288
0.0349
0.0411
0.0473
0.536
0.0600
0.0664
0.0729
0.0794
0.0860
0.0926
0.0994
0.1061
0.1130
0.1198
29
Table 3.1. Continued
Time (hours)
20
21
22
23
24
25
26
27
28
29
30
ML -Run 1
0.1303
0.1373
0.1443
0.1512
0.1582
0.1652
0.172
0.1791
0.1861
0.1930
0.2
ML - Run 2
0.1208
0.1270
0.1333
0.1396
0.1459
0.1529
0.1598
0.1668
0.1742
0.1815
0.1888
ML -Run 3
0.1291
0.1368
0.1444
0.1521
0.1597
0.1702
0.1785
0.1862
0.1938
0.2018
0.2098
Average ML
0.1267
0.1337
0.1407
0.1476
0.1546
0.1628
0.1701
0.1774
0.1847
0.1922
0.1995
ML from fitted curve
0.1268
0.1338
0.1409
0.1480
0.1552
0.1624
0.1698
0.1771
0.1846
0.1920
0.1996
30
0,25 Actual d i t i points Fitted curve
10 15 20 Corrosion time (hours)
25 30
Figure 3.1: Corrosion mass loss versus Time
31
3.2 Tensile Test Results
The tensile tests were done to estimate the ultimate tensile sttength of Al-7075
T6 aUoy. Table 3.2 shows the results of the tests.
Table 3.2: Tensile test data for A1-7075-T6
Test run
1
2
3
Ultimate tensile sttength (psi)
82,000
81,500
82,670
Average ultimate tensile sttength (psi)
82,056
3.3 Fatigue Test Results
The results of the fatigue tests for the specunens that were cold expanded prior to
corrosion are shown in Table 3.3. Figure 3.2 shows a graphical representation of the data
in Table 3.3.
Figure 3.2 shows that non-cold expanded specimens widi 0% corrosion have an
average fatigue Ufe of approximately 97,000 cycles and as the specmiens are corroded the
fatigue life reduces drasticaUy. At 10% corrosion, die fatigue Ufe of the specmiens is
around 23,000 cycles and at 20% corrosion it is approxunately 14,000 cycles. The data
shows that fatigue Ufe of die specunens decreases exponentially widi increased corrosion.
When the holes in die un-corroded specimens were cold expanded by 2%, die
specimens did not break tiU 2,000,000 cycles at which point die tests were stopped. For
32
calculation purposes, die fatigue Ufe of die specimens was recorded as 2,000,000 cycles.
When die cold expanded specimens were corroded to 10% mass loss, die specimens
fractured at approximately 470,000 cycles. The test data shows diat 2% cold expansion
of die holes improves die fatigue Ufe of die specunens nearly twenty tunes when diey are
corroded to 0% or 10% mass loss. At 20% mass loss level, die effects of 2% cold
expansion on die fatigue life were negUgible and die specimens fractured at around
25,000 cycles.
When the holes in the specimens were subjected to 4% cold expansion, the
specimens did not fracture tiU 2,000,000 cycles for bodi 0% and 10% mass loss levels.
The fatigue test data shows that 4% cold expansion improved die fatigue Ufe of the
specimens approximately four times compared to 2% cold expansion. However, at 20%
mass loss level, the specimens fractured at around 42,000 cycles and the effects of 4 %
cold expansion were minimal. The fatigue ttend Unes for cold expanded specimens show
a drastic reduction in the fatigue life of the specunens with corrosion implying that
corrosion has an exponential effect on the fatigue Ufe of cold expanded specimens. Table
3.4 and Figure 3.3 show the fatigue test data for specimens that were corroded prior to
cold expansion.
Figure 3.4 gives a comparison of the fatigue Ufe for the specimens that were given
2% cold expansion prior to corrosion and the specunens cold expanded after corrosion.
The graph clearly shows that the fatigue life of the specunens that were cold expanded
after corrosion is lower than the fatigue life of specimens that were cold expanded before
corrosion. This effect is particularly visible at 10% corrosion level. The specimens that
33
Table 3.3: Fatigue test data for cold expanded specimens subjected to subsequent corrosion
Cold expansion
Corrosion (% mass loss)
Cycles to Failure Mean cycles to failure Standard deviation
10
20
10
20
10
20
97,457 100,214 88,740
24,389 22,329 23,910 24,109
14,208 16,804 11,300 14,738
> 2,000,000 > 2,000,000 > 2,000,000
430,352
1,300,214 482,502 493,278
29,322 23,501 24,672
> 2,000,000 > 2,000,000 > 2,000,000
1,720,463 > 2,000,000 > 2,000,000
38,701 45,128 43,125 42,108
95,470
23,684
14,217
> 2,000,000
468,710
25,831
> 2,000,000
> 1,906,821
42,265
1,2,3: specimen did not break and the test was stopped at this point * reading was not included while calculating the mean and standard deviation
5989
920
2273
33654
3079
161390
2608
34
2,5
2 4 6 8 10 12 14 16 18 20 Mass loss due to corrosion (%)
Figure 3.2: Fatigue life of cold expanded (CET) specimens subjected to subsequent corrosion.
35
Table 3.4: Fatigue test data for corroded specimens subjected to subsequent cold expansion
Corrosion „ , _ ,, Mean cycles to c^. •, • • • ^ ,„ , , expansion Cycles to Failure ^ ., Standard deviation (% mass loss) ., failure
97,457 0 0 100,214 95,470'* 5989
88,740
> 2,000,000 > 2,000,000 > 2,000,000
> 2,000,000 > 2,000,000 > 2,000,000
20
> 2,000,000 > 2,000,000 ''^
> 2,000,000 > 2,000,000 ''•'
24,389
10 0 23'9?0 ^^'^^^' ^^° 24,109
351,439
10 2 300,209 337,750 25,293 ^" ^ 345,320
354,035
> 2,000,000 > 2,000,000 > 2,000,000
10 4 > 2,000,000 > 2,000,000'°
14,208
14,738
42,814 24,636 29,648 8084
^ 24,232 25,908
28,904
? 6 m " '"^ ''"•
4,5,7,9,11: same values used in Table 3.3 6, 8,10: specimen did not break and the test had to be stopped at this point
36
6 8 10 12 14 Mass loss due to corrosion (%)
Figure 3.3: Fatigue Ufe of corroded specimens subjected to subsequent cold expansion(CET).
37
were cold expanded prior to corrosion have a fatigue Ufe of around 468,710 cycles while
the specimens that were cold expanded after corrosion have a fatigue Ufe of 337,750
cycles. At 0%, 20% corrosion levels the fatigue Ufe of the specimens for both the cases
was almost the same. Figure 3.5 shows the fatigue life graphs at 4 % cold expansion for
the specimens cold expanded prior to corrosion auid specimens corroded before cold
expansion. In this case the fatigue Ufe of the specimens for both the cases was identical as
can be seen from the graphs.
3.4 Statistical Analysis
Statistical analysis was done to study the effect of variables involved, namely cold
expansion, corrosion and the order of cold expansion on the fatigue Ufe of the specimen.
This was done by using Analysis Of Variance (ANOVA) procedure. ANOVA procedure
was performed for balanced and unbalanced 3^ and 3^x2' Factorial designs using
ANOVA and GLM subroutines in SAS. The results of die analysis are discussed here.
38
2.5
CD
o
•i -̂̂ to
(0
o >. o
E 0.5
XV.
XX ^X ^X xX xX x^ X
1 1 —— Fitted curve for specimen cold expanded first ' 1- — - Fitted curve for specimen corroded first ' ; • Actual data point for specimen cold expanded first | ' , Q Actual data point for specimen corroded first
X X . X X.
X X. X >w "X > v
X X. X X.
X X "X X.
X >v X X , X X
X X
N X ^ V
'
^ ^ 1 X nx .
^ ̂ ̂ __ — , - « 2 4 6 8 10 12 14 16 18 20
Mass loss due to corrosion (grams)
Figure 3.4: Comparison of fatigue life of specimens cold expanded prior to corrosion and specimens cold expanded after corrosion at cold expansion (CET) = 2%
39
2,5
g Fitted curve for specimen cold expanded first Fitted curve for specimen corroded first Actual data points for specimen corroded first actual data points for specimen cold expanded first
6 8 10 12 14 Mass loss due to corrosion (grams)
20
Figure 3.5: Comparison of fatigue Ufe of specunens cold expanded prior to corrosion and specunens cold expanded after corrosion at cold expansion (CET) = 4 %. Curves are almost similar.
40
3.4.1 ANOVA for 3^ factorial design
Fatigue test data from Table 3.3 were used for analyzing die effect of cold
expansion and corrosion on die fatigue Ufe of die specimen. Table 3.5 shows die data
used for analysis for balanced3^ factorial design. Table 3.6 shows die results of die
ANOVA analysis.
The results show that cold expansion and corrosion have a significant effect on
the fatigue Ufe of the specimen, and there is a significant interaction between cold
expansion and corrosion. This can be inferred from the high F-values and low P-values
for cold expansion and corrosion. The results also show that corrosion is a sUghdy more
dominant factor compared to cold expansion.
Table 3.7 shows the data used for the unbalanced 3^ factorial design. The results
of this analysis shown in Table 3.8 and Table 3.9 further confirm the results discussed
above.
41
Table 3.5: Fatigue Ufe data for balanced 3^ factorial design
Cold expansion (%)
0
2
4
Corrosion (%) 0
97,457 100,214 88,740
2,000,000 2,000,000 2,000,000
2,000,000 2,000,000 2,000,000
10
24,389 22,329 23,910
430,352 482,502 493,278
1,720,463 2,000,000 2,000,000
20
14,028 16,804 11,300
29,322 23,501 24,672
38,701 45,128 43,125
42
Table 3.6: ANOVA for balanced 3^ factorial design
Source of variation
Model
Cold expansion
Corrosion
Cold expansion
* Corrosion
Error
Corrected total
Degree of freedom
8
2
2
4
18
26
Sum of squares
2.095 e 13
7.629 e 12
8.276 e 12
5.050 e 12
5.282 e l l
2.148 e 13
Mean square
2.619 e 12
3.814 e 12
4.138 e 12
1.263 e 12
2.934 e 10
F-value
89.26
129.98
141.02
43.02
-
-
P-value
< .0001
< .0001
< .0001
< .0001
-
43
Table 3.7: Fatigue life data for unbalanced 3^ factorial design
Cold expansion (%)
0
2
4
Corrosion (%) 0
97,457 100,214 88,740
2,000,000 2,000,000 2,000,000
2,000,000 2,000,000 2,000,000
10
24,389 22,329 23,910 24109
430,352 1,300,214 482,502 493,278
1,720,463 2,000,000 2,000,000
20
14,028 16,804 11,300 14,738
29,322 23,501 24,672
38,701 45,128 43,125 42,108
44
Table 3.8: ANOVA for unbalanced 3^ factorial design (Type I)
Source of variation
Model
Cold expansion
Corrosion
Cold expansion
*
Corrosion
Error
Corrected total
Degree of freedom
8
2
2
4
22
30
Type I sum of squares
2.2401 e 13
7.491 e 12
8.911 e 12
5.997 e 12
5.7304 e l l
2.297 e 13
Mean square
2.8001 e 12
3.746 e 12
4.456 e 12
1.499 e 12
2.6047 e 10
-
F-value
107.50
143.82
171.07
57.56
-
P-value
< .0001
< .0001
< .0001
< .0001
-
-
45
Table 3.9: ANOVA for unbalanced 3^ factorial design (Type III)
Source of variation
Model
Cold expansion
Corrosion
Cold expansion
* Corrosion
Error
Corrected total
Degree of freedom
8
2
2
4
22
30
Type III sum of squares
2.2401 e 13
8.738 e 12
9.166 e 12
5.997 e 12
5.7304 e l l
2.297 e 13
Mean square
2.8001 e 12
4.368 e 12
4.583 e 12
1.499 e 12
2.6047 e 10
F-value
107.50
167.73
175.95
57.56
P-value
< .0001
< .0001
< .0001
< .0001
-
-
46
3.4.2 ANOVA for 3 ' x 2' Factorial designs
Fatigue test data from Table 3.3 and Table 3.4 were used for analyzing die effects
of cold expansion, corrosion and the order of cold expansion on the fatigue life of die
specimen. Table 3.10 shows die data used for 3^x2' factorial analysis and Table 3.12
shows the results of the ANOVA analysis.
The results show that corrosion and cold expansion have a significant effect on
the fatigue life of die specimen. This can be inferred from the high F-values. Corrosion
has a F- value of 556 while cold expansion has a F-value of 516. The F-values also show
that corrosion is a more dominant factor when compared to cold expansion. The order of
cold expansion has only a sUght effect on the fatigue life of the specimen compared to
corrosion and cold expansion. This can be inferred from the low F-value of 1.17 and high
P-value of 0.2857. The results also show that there is a significant amount of interaction
between corrosion and cold expansion. The low F-values show that there is not much
interaction between cold expansion and the order of cold expansion and between
corrosion and the order of cold expansion.
Table 3.12 shows die data for unbalanced 3^ x2^ factorial design, and Table 3.13
and Table 3.14 show the results of the ANOVA analysis. The results confirm die
observation made above.
47
Table 3.10: Fatigue Ufe data for balanced 3^ x 2' factorial design
Cold expansion
(%)
0
2
4
Order of treatment A
Corrosion (%) 0
97,457 100,214 88,740
2,000,000 2,000,000 2,000,000
2,000,000 2,000,000 2,000,000
10
24,389 22,329 23,910
430,352 482,502 493,278
1,720,463 2,000,000 2,000,000
20
14,028 16,804 11,300
29,322 23,501 24,672
38,701 45,128 43,125
B Corrosion (%)
0
97,457 100,214 88,740
2,000,000 2,000,000 2,000,000
2,000,000 2,000,000 2,000,000
10
24,389 22,329 23,910
351,439 345,320 354,035
2,000,000 2,000,000 2,000,000
20
14,028 16,804 11,300
25,636 24,232 25,906
28,908 27,310 26,001
48
Table 3.11: ANOVA for balanced 3^x2' factorial design
Source of variation
Model
Cold expansion
Order
Corrosion
Cold expansion * Order
Cold expansion * Corrosion
Order* Corrosion
Cold expansion * Order * Corrosion
Error
Corrected total
Degree of freedom
17
2
1
2
2
4
2
4
36
53
Sum of squares
4.315 e 13
1.520 e 13
1.729 e 10
1.639 e 13
6.589 e 10
1.131 e 13
3.149 e 10
1.452 e l l
5.301 e l l
4.3683 e 13
Mean square
2.538 e 12
7.600 e 12
1.729 e 10
8.193 e 12
3.295 e 10
2.827 e 12
1.574 e 10
3.630 e 10
1.472 e 10
F-value
172.39
516.10
1.17
556.43
2.24
191.96
1.07
2.47
P-value
< .0001
< .0001
0.2857
< .0001
0.1214
< .0001
0.3539
0.0624
-
49
Table 3.12: Fatigue Ufe data for unbalanced 3^ x2 ' factorial design
Cold expansion
(%)
0
2
4
Order of treatment A
Corrosion (%) 0
97,457 100,214 88,740
2,000,000 2,000,000 2,000,000
2,000,000 2,000,000 2,000,000
10
24,389 22,329 23,910 24,109
430,352 1,300,2214
482,502 493,278
1,720,463 2,000,000 2,000,000
20
14,028 16,804 11,300 14,738
29,322 23,501 24,672
38,701 45,128 43,125 42,108
B Corrosion (%)
0
97,457 100,214 88,740
2,000,000 2,000,000 2,000,000
2,000,000 2,000,000 2,000,000
10
24,389 22,329 23,910 24,109
351,439 300,209 345,320 354,035
2,000,000 2,000,000 2,000,000
20
14,028 16,804 11,300 14,738
42,814 25,636 24,232-25,906
28,908 27,310 26,001
50
Table 3.13: ANOVA for unbalanced 3^ x2 ' factorial design (Type I)
Source of variation
Model
Cold expansion
Order
Corrosion
Cold expansion * Order
Cold expansion * Corrosion
Order * Corrosion
Cold expansion * Order * Corrosion
Error
Corrected total
Degree of freedom
17
2
1
2
2
4
2
4
44
61
Type I sum of squares
4.602 e 13
1.561 e 13
6.495 e 9
1.725 e 13
1.278 e l l
1.287 e 13
2.852 e 10
1.254 e l l
5.752 e l l
4.6599 e 13
Mean square
2.707 e 12
7.806 e 12
6.495 e 9
8.625 e 12
6.380 e 10
3.218 e 12
1.426 e 10
3.134 e 10
1.307 e 10
F-value
207.06
597.03
0.50
659.69
4.88
246.16
1.09
2.40
-
P-value
< .0001
< .0001
0.4846
< .0001
0.0122
< .0001
0.3449
0.0645
51
Table 3.14: ANOVA for unbalanced 3 ' x2 ' factorial design (Type III)
Source of variation
Model
Cold expansion
Order
Corrosion
Cold expansion * Order
Cold expansion * Corrosion
Order * Corrosion
Cold expansion * Order * Corrosion
Error
Corrected total
Degree of freedom
17
2
1
2
2
4
2
4
44
61
Type III sum of squares
4.602 e 13
1.715 e 13
1.236 e 10
1.814e 13
5.394 e 10
1.288 e 13
2.232 e 10
1.254 e l l
5.752 e l l
4.6599 e 13
Mean square
2.707 e 12
8.574 e 12
1.236 e 10
9.071 e 12
2.697 e 10
3.219 e 12
1.116elO
3.134 e 10
1.307 e 10
F-value
207.06
655.80
0.95
693.77
2.06
246.22
0.85
2.40
-
-
P-value
< .0001
< .0001
0.3362
< .0001
0.1392
< .0001
0.4328
0.0645
52
3.5. Fractographic Analysis Results
Fractographic analysis was done for (0,0), (0,10), (2,10), (2,20), (4,20) specmiens
from fatigue test. The remaining specimens namely, (2,0), (4,0), (4,10) were not
examined as they did not fracture. Results of the analysis are discussed below.
3.5.1. (0.0) specimen
Figure 3.6 shows the appearance of the edges of an un-corroded, non-cold
expanded specimen. Figure 3.6a shows the comer and 3.6b shows the edge of the hole.
In the figure the edges of the specimen are clearly defined and do not show any damage
other than that due to fracture
Figure 3.7 shows the variation in the pattern seen on the fracture surface along the
length of the specimen. Near the hole, the fracture surface has a bright and shiny
appearance and shows cleavage fracture type features. This can be seen in Figure 3.7a.
As the crack propagates, the surface shows features that are characteristics of ductile
fracture. Figure 3.7b shows a surface similar to the previous one except for the presence
of some voids, which are characteristic of ductile fracture. Further along the length, the
fracture becomes quasi-cleavage type, showing features associated with both cleavage
and ductile fractures. This can be seen in Figure 3.7c, in which the surface shows a
number of dimples along with some cleavage fracture features. Further along the length,
the fracture becomes completely ductile as seen in Figure 3.7d. The same pattern is
repeated on the other end of the hole.
53
.'.»&
, ^ C -'•̂
. • : 1 ^ - : « ; \ ^ * •/•' ^ i _ . . / '
000101 12KV X£50""i£0Ufti
(a)
J00r07 12KV X780
(b)
880132 leKV Xe.80K 15,0Uin
(c)
Figure 3.6: Appearance of the edge of a (0,0) specimen, (a) Comer of specimen near the hole, (b) Edge of the specimen near the hole, (c) Side edge of the specimen at a distance 0.1 inch from the hole. The surface shows no damage other than due to fracture.
54
•̂WJ
008103 Ic'KV >i700 43i.
(a) (b)
(c) (d)
Figure 3.7: Appearance of the surface along the length of the (0,0) specimen, (a) Cleavage fracture type surface near the edge, (b) Cleavage Fracture type surface at a distance of 0.1 inch from the hole. In addition some voids can be seen on the surface, (c) Fracture surface at a distance of 0.3 inches from hole showing quasi-cleavage fracture pattern, (d) Fracture surface at a distance of 0.5 inches from hole showing ductile fracture pattem.
55
Figure 3.8 shows the striations formed due to fatigue testing on the surface of the
specimen. Near the hole no striations were observed as shown in Figure 3.8a. As die
crack propagates the striations become increasingly visible and larger as can be seen in
Figures 3.8b, c, d and e. In Figure 3.8b taken at distance of 0.05 inches from die hole die
striations could be seen only at a magnification of around 5000, while at a distance of 0.3
inches from the hole the striations were visible at a magnification of 2000. Near the
ductile region no striations were observed as seen in Figure 3.8f
3.5.2. (0.10) specimen
Figure 3.9 shows the corroded surface of the specimen near the hole. Figure 3.9a
shows the edge of the hole. The figure shows ridges along the edge, which represent the
source of the crack. The edges here show some damage due to corrosion as can be seen in
Figures 3.9a and b. The fracture and striation pattems seen here were similar to the
patterns observed in the (0,0) specimen.
3.5.3 (2.10) specimen
This specimen showed the same features as seen in the other two specimens.
Figure 3.10 shows the corroded edge near to the hole. Figure 3.10a shows the edge close
to the hole. The figure shows a number of ridges on die edge, which represent the source
of the crack.
56
(a) (b)
(c) (d)
Figure 3.8: Fatigue striations for (0,0) specimen, (a) No striations are seen near the hole, (b) Striations at a distance of 0.05 inches from the hole, (c) Striations at a distance of 0.1 inch from the hole, (d) Striations at a distance of 0.2 inches from the hole. Fatigue striations become increasingly larger as the crack propagates.
57
668134 1£KV X S . 8 8 K " i s l S u m
(e) (f)
Figure 3.8 (continued): (e) Striations at a distance 0.3 inches from die hole, (f) No striations could be seen in ductile fracture region
^^-f*J>.V*^ •t! -
800138 12KV x e e i e ' .50ISII1
(a) (b)
Figure 3.9: Appearance of edges of (0,10) specimen, (a) Edge of the hole, (b) Comer of the hole. They show extensive damage due to corrosion compared to Figure 3.6.
58
On closer observation of the corroded surface, a number of secondary cracks
could be seen near die hole. This is shown in Figure 3.10b. Figure 3.10c shows a higher
magnification image of die corroded surface. The figure shows sharp cracks formed on
the surface due to corrosion, similar to intergranular fracture.
Figure 3.11 shows the fracture pattem formed on the surface due to the
appUcation of cycUc load. The pattem seen here was sunilar to one seen in (0,0)
specimen. Figure 3.11a shows the cleavage fracture region, while Figure 3.11b shows the
ductile fracture. The specimen showed a gradual transition from cleavage to ductile
fracture on one side of the hole. The other side had only ductile fracture pattem. Figure
3.12 shows the fatigue pattem formed on the surface due to cycUc loading on the other
side of the hole. Fatigue striations seen here were similar to one observed in (0,0)
specimen.
3.5.4 (2.201 specimen
Figure 3.13 shows the corroded surface of the specimen. The surface of the
specimen was more severely damaged when compared to a 10% corrosion specimen.
Figure 3.13a shows the edge of die hole. Figures 3.13a, b and c show widespread damage
to the specunen along die sides. Figures 3.13b and c show die damage on die waUs of die
hole due to corrosion and fatigue cracking. The fracture pattem formed on die surface of
the specunen is sunilar to one formed on die (2,10) specunen. The surface shows a
gradual transition from cleavage to ductile fracture on one side of die hole, while on die
other side it undergoes only ductile fracture as in (2,10) specunen.
59
3.5.5 (4.20) specimen
Figure 3.14 shows die corroded surface of die specimen close to the edge. Unlike
odier specimens, large cracks Uke die one shown in Figure 3.14b were observed in (4,20)
specimen. These cracks were found to originate near the hole and ran through the enter
length of the specimen. Figures 3.14c also shows a number of secondary cracks formed
near the edges, which were corroded.
Also, die (4,20) specimen showed brittle fracture region away from the edge of
the hole. Figures 3.15a and b show surfaces having cleavage fracture pattems in the midst
of ductile fracture regions (Figure 3.15c and d). On the other side there was a gradual
transition from cleavage to ductile fracture as seen in Figure 3.16 .
60
•m^.'s^^t..'-^^.
^ \
066103 12KV X1.00K 30uir.
(a) (b)
000104 12KV X2.50K 12.0uffi
(C)
Figure 3.10: Corroded edge for (2,10) specimen, (a) Edge of the hole, (b) Edge at a higher magnification, (c) lUgher magnification image of the crack Edge and surface close to the hole show number of cracks, which were not seen in (0,0) specimen.
61
000111 12KV X680 50UB 088131 12KV xsee
(a) (b)
Figure 3.11: Appearance of the fracture surface for (2,10) specimen, (a) Cleavage type fracture pattem near the hole, (b) Ductile fracture type pattem at a distance of 0.4 inches from the hole. There is a gradual transition from cleavage type fracture to ductile fracture.
860128 12KV X500"
(a) (b)
Figure 3.12: Appearance of die fracture surface for (2,10) specunen on die odier side of the hole, (a) Ductile fracture type pattem near die hole, (b) Ductile fracture type pattem at a distance of 0.4 inches from die hole. Dunples get elongated as die crack propagates.
62
(a) (b)
080105 12KV X1.50K 29.Sum
(c)
Figure 3.13: Corroded edge for (2,20) specimen, (a) Edge of the hole, (b) Higher magnification image of the edge of the hole, (c) Higher magnification image of the surface of the hole. Side waUs of the hole show extensive cracking.
63
(a) (b)
000121 12KV X500 60um
(C)
Figure 3.14: Corroded edge for (4,20) specimen, (a) Near the hole, (b) Crack on the surface, (c) Surface near the comer of the hole shows number of smaUer cracks.
64
e s e i i s 12KV K50e"
(a) (b)
(c) (d)
Figure 3.15: Surface on the left side of the hole for (4,20) specimen, (a) shows a flat region similar to cleavage fracture region, (b) Higher magnification image of the same, (c) Shows ductile fracture region around the cleavage fracture region, (d) Higher magnification image of the same. Cleavage fracture region was found away from the hole and was surrounded by ductile fracture region.
65
000143 I2KV X500 ekun,
(a) (b)
006147 12KV X580
(C) (d)
Figure 3.19: Appearance of the surface on die right hand side of die hole for (4,20) specimen, (a) Cleavage fracture pattem near the edge, (b) Cleavage fracture pattem at a distance of 0.05 inches from the hole, (c) Quasi-cleavage fracture pattern at a distance of 0.15 inches from the hole, (d) Ductile fracture pattem at a distance of 0.4 inches from the hole. The surface shows a gradual ttansition from cleavage fracture to ductile fracture.
66
CHAPTER IV
CONCLUSIONS AND RECOMMENDATIONS
4.1 Conclusions
The following conclusions were drawn from the study.
1. Cold expansion of specimens proved to be an effective means of enhancing the
fatigue life of the specimens. The benchmark specimens that were not subjected to cold
expansion, or corrosion, showed an average fatigue life of 95,500 cycles. 2% cold
expansion of specimens resulted in a 20-fold improvement in the fatigue life of
benchmark specimens. These specimens had an average fatigue life of over 2,000,000
cycles. Higher cold expansion of 4% also showed improvements in fatigue life of
specimens beyond 2,000,000 cycles.
2, Corrosion as measured by percentage mass loss of the specimens, resulted in a
reduction in the fatigue life of the specimens. In benchmark specimens, 10% corrosion
resulted in the reduction of fatigue life to 23,700 cycles from 95,500 cycles. The effect of
corrosion was also apparent in cold expanded specimens. The fatigue life of 2% cold
expanded specimens dropped from over 2,000,000 cycles to 468,700 cycles after a mass
loss of 10% due to corrosion. However, the fatigue life of 4% cold expansion specimens
oidy dropped from over 2,000,000 cycles to 1,900,000 cycles after a 10% mass loss due
to corrosion. This data clearly shows that higher cold expansion provides more resistance
against fatigue failure, even when the material is subjected to a subsequent corrosion. The
data also shows that 10% corrosion causes the fatigue life of non-cold expanded
67
specimens to be reduced by a factor of 4. The same observation can be made regarding
2% cold expansion specimens where 10% corrosion results in a 4-fold reduction in the
specimens fatigue life.
3. Two independent mechanisms contribute to the observed reduction in the
fatigue Ufe of the corroded specimens. Ffrst is the obvious reduction in the materials
cross sectional area which gives rise to higher sttess ampUtudes and hence lowered
fatigue life. The second mechanism has to do widi stress corrosion cracking (SCC), a
phenomenon where die effect of corrosion is accentuated by the presence of a stress field.
It is not clear at this point how much of the above reduction is due to the decrease in
materials cross sectional area, and how much of the reduction is due to degradation of the
material properties due to corrosion. Further studies are requfred in this area to
understand it clearly.
4. The effect of higher mass loss due to corrosion, as expected, was further
reduction in the fatigue life of the specimens. For benchmark specimens, the fatigue life
was reduced from 95,500 cycles to 14,200 cycles for 20% corroded specimens as
compared to 23,700 cycles for 10% corroded specunens. At higher corrosion rates die
effect of cold expansion on the fatigue life of die specimens was also negUgible. 2% cold
expansion specimens subjected to 20% mass loss fractured at around 26,000 cycles while
4% cold expansion specmiens subjected to 20% mass loss fracttued at around 42,000
cycles. Again, it is not clear at tins point how much of die above reduction in fatigue life
is due to die decrease in materials cross sectional area, and how much of die reduction is
due to degradation of die material properties due to corrosion itself.
68
5. The data from Table 3.4 also indicates that cold expansion can dramatically
increase the fatigue Ufe of specimens, which have been afready corroded. A 2% cold
expansion of 10% corroded specimen, increased its fatigue life from 23,700 cycles to
337,800 cycles. Cold expansion of the same specimen by 4% resulted in a fatigue life
improvement beyond 2,000,000 cycles. One observation here is that in general the fatigue
life of a specimen was higher if the cold expansion was done before the corrosion than if
the cold expansion was done after corrosion. This data supports the theory that the
material properties in the corroded zone undergo a degradation, which when foUowed by
cold expansion, will produce an adverse effect on the abiUty of the material to resist crack
propagation.
4.2 Recommendations
Corrosion of specimens in this study was conducted to simulate envfronmental
effects on a material operating in a corrosive envfronment. However in die real world,
corrosion occurs simultaneously with die cycUc loading on die material. Therefore in an
ideal case, corrosion of the material should occur as die material is cycUcaUy loaded.
ReaUzing the difficulties associated widi conducting such an experiment, an alternative
approach for futtu-e sttidies might be to intermpt die corrosion cycle periodically,
foUowed by cycUcaUy loading die specimen to 10% of its expected Ufe, foUowed by
anodier increment of corrosion, foUowed by anodier increment of cycUc loading, and so
on until the specimen fractures.
69
Also, just as it has been shown that cold expansion can be beneficial during
various stages of a components fatigue Ufe (Gaerke et al., 2000), it would be interesting
to study the effect of cold expansion at different intervals during the corrosion cycle. For
example, if a specimen is to be corroded by 10% and then cold expanded by 2%, it would
be interesting to stop the corrosion at 2%, 4%, 6% and 8% (in four different specimens),
conduct a 2% cold expansion, and continue the corrosion process to a total of 10%. Such
a study will show the effect of cold expansion timing on the corrosion evolution.
70
REFERENCES
Anderson, T.L., 1995, Fracture Mechanics - Fundamentals and Applications, 2""^ Edition, CRC Press Inc., Boca Raton, FL.
ASM Handbook, vol 13, Corrosion, 1987, ASM fritemational, U.S.A.
ASTM Gl-90 standard, 1994, Standard Practice for Preparing, Cleaning and Evaluating Corrosion Test Specimens, American Society for Testing and Materials Philadelphia, PA.
ASTM G31-72 standard, 1994, Standard Practice for Laboratory Immersion Corrosion Testing of Metals, American Society for Testing and Materials, Philadelphia, PA.
ASTM special technical pubUcation, 1966, Stress Corrosion Testing, American Society for Testing and Materials, Philadelphia, PA.
Baboian, R., (Ed.), 1995, Corrosion Tests and Standards: Application and Interpretation, American Society for Testing and Materials, Philadelphia, PA.
Chen, G.S., Wan, K.C., Gao, M., Wei, R.P., Floumey, T.H., 1996, "Transition from Pitting to Fatigue Crack Growth- Modelling of Corrosion Fatigue Crack Nucleation in Al-2024 T6 AUoy," Material Science & Engineering A: Structural Materials Properties, Microstructure and Processing, V-219, n 1-2, pp 126-132.
Chandawanich, N., Sharpe, W., 1979, "Experimental Sttidy of Fatigue Crack Initiation and Growth from Cold Worked Holes," Engineering Fracture Mechanics, V-11, n-4, pp 609-620.
Cook, R., GUnos, N., Wagstaff, P., 1996, "The Effect of Surface Corrosion on Fatigue Behavior of Aluminum AUoy Specimen Containing Cold Expanded Holes," Proceedings of the 2(f^ ICAS Congress, Sorrento.
Cook, R., GUnos, N., Wagstaff, P., 1999, "Role of Surface Pitting Corrosion on Effectiveness of Hole Cold Expansion," RTO Meeting Proceedings, Corfa, Greece.
Davis, J.R., (Ed.), 1999, Corrosion of Aluminum and Aluminum Alloys, ASM, OH.
Dutta, N.,1997, "Analytical, Numerical, and Experimental Investigations of Elastic-Plastic Boundary and Residual Stress Field Around a Cold-Expanded Hole," PhD Dissertation, Texas Tech University, TX.
71
Dutta, N., Rasty, J., and Rassaian, M., 1997, "Finite Element Analysis of Elastic-Plastic Zone Around Cold-Expanded Holes," Post-Conference Proceedings of the 1997 Society for Experimental Mechanics (SEM) Spring Conference, June 2-5, 1997, Bellevue, Washington, pp. 108-115.
Dutta, N., Rasty, J., 1999, "Determination of Elastic-Plastic Boundary Condition Around Cold-Expanded Holes using Elastic Strain," Proceedings of the 1999 Society of Experimental Mechanics (SEM) Spring Conference, June 7-9, 1999, Cincinnati, OH.
Fong, J.T., (Ed.), 1978, Fatigue Mechanism, American Society for Testing and Materials, Philadelphia, PA.
Fong, J.T., Fields, R.J., (Ed.), 1988, Basic Questions in Fatigue, American Society for Testing and Materials, Philadelphia, PA.
Gaerke, j . , Zhang, X., Wang, Z., 2000, "Life Enhancement of Fatigue-Aged Fastener Holes Using Cold Expansion Process," Journal of Aerospace Engineering, V-214, n 5, pp 281-293.
Gilbertson, L.N., Zipp, R.D., (Ed.), 1979, Fractography and Material Science, American Society for Testing and Materials, Philadelphia, PA.
HuU, D., 1999, Fractography- Observing, Measuring and Interpreting Fracture Surface Topography, T' Edition, Cambridge University Press, Cambridge, U.K.
Moesser, M., EUiot, C.B., Kinyon, S., Houmoy, T., 1995, "The Role of Frettmg Corrosion and Fretting Fatigue m Afrcraft Rivet Hole Cracking," Proceedings of the Symposium -International Committee on Aeronautical Fatigue, V-18A^2, pp 1053-1068.
Montgomery, D.C., 2001, Design and Analysis of Experiments, 5*̂ Edition, John Wiley & Sons, Inc., New York.
Moshier, M.A., Hilberry, B.M., 1998, "Inclusion of Compressive Residual SQ-ess Effects in Crack Growdi ModeUng," Fatigue and Fracture of Engineering Materials and Structures, v-22, n-6, pp 519-526.
Obert, B.D., 2000, "Quantification of Corrosion in Al 7075 T6 Aluminum AUoy," ' Master's Thesis, Texas Tech University, TX.
Oldham, H.B., Myland, J.C, 1994, Fundamentals of Electro Chemical Science, l" Edition, Academic Press, San Diego, CA.
72
Ozdemfr, A.T., Edwards, L., 1996, "Measurement of the Three Dimensional Residual Stress Distribution Around SpUt Sleeve Cold Expanded Holes," Journal of Strain Analysis for Engineering Design, v-31, n-6, pp 413-421.
Pavier, M.J., Poussard, C.G.C., Smidi, D.J., 1997, "A Finite Element Simulation of die Cold Working Process for Fastener Holes," The Journal of Strain Analysis for Engineering Design, n-b-4, pp 287-300.
Petrak, G.J., Stewart, R.P., 1976, "Retardation of Crack Emanating from Fastener Holes," Engineering Fracture Mechanics, v-6, pp 275-282.
PhilUps, J.L., 1973, "Fatigue Improvement by Sleeve Cold Working," National Aerospace Engineering and Manufacturing Meeting, Los Angles, CA.
Phillips, J.L., 1974, "Sleeve Cold Working of Fastener Holes," Afr Force Materials Laboratory Report AFML - TR - 74 -10, v-1.
Rachid, G., Shi, H.J., Guo, R., Mesmacque, G., 2000, "Effects of Expanded and Non-Expanded Hole on the Delay of Arresting Crack Propagation for Aluminum AUoy," Material Science & Engineering A: Structural Materials Properties, Microstructure and Processing, V-286, n 2, pp 244-249.
Reid, L., 1993, "SpUt Sleeve Cold Expansion as a Rework Process for Previously Cold Expanded Holes," Presented at ICAF, Stockholm, Sweden.
Reid, L., 1997, "Incorporating Hole Cold Expansion to Meet DurabiUty and Damage Tolerance Airworthiness Objectives," SAE Afr Frame and Engine Maintenance and Repafr Conference, Vancouver, Canada.
Rufin, A.C., 1993, "Extending Fatigue Life of Afr Craft Engine Components by Hole Cold Expansion Technology," Journal of Engine for Gas Turbines & Power, ASME, v-115, n-1, pp-165-171.
Sankaran, K.K., Perez, R., lata, K.V., 2001, "Effects of Pitting Corrosion on die Fatigue Behavior of Aluminum AUoy 7075 T6: ModeUng and Experunental Sttidies," Material Science and Engineering, v-297, n 1-2, pp 223-229.
Stirauss, B.M., CuUen, W.H., (Ed.), 1977, Fractography in Failure Analysis, American Society for Testing and Materials, Philadelphia.
73
PERMISSION TO COPY
In presenting this thesis m partial fulfUlment of the requuements for a master's
degree at Texas Tech University or Texas Tech University Health Sciences Center, I
agree that the Library and my major department shaU make it freely avadable for
research purposes. Permission to copy this thesis for scholarly purposes may be
granted by the Dfrector of the Library or my major professor. It is understood that
any copying or publication of this thesis for financial gain shaU not be aUowed
without my flirther written permission and that any user may be liable for copyright
mfruigement.
Agree (Permission is granted)
Student Signature Date
Disagree (Permission is not granted.)
Student Signature Date