Download - Weld Defect & Repair,Ham
-
8/16/2019 Weld Defect & Repair,Ham
1/40
Welding InspectionDefects/Repairs
-
8/16/2019 Weld Defect & Repair,Ham
2/40
Cracks
Solid inclusions
Surface and profiles
Misalignment (set-up
irregularities)
Gas pores and porosity
Weld DefectsWeld Defects
Lack of fusion
Incomplete enetration
Incomplete !usion
"urn #$roug$
Internal Conca%ity
-
8/16/2019 Weld Defect & Repair,Ham
3/40
CracksCracks
-
8/16/2019 Weld Defect & Repair,Ham
4/40
Classified by Shape
Longitudinal
#rans%erse
Classified by Position
&' Centreline
Crater
!usion one
arent metal
CracksCracksCracks t$at may occur in *elded materials are caused
generally +y many factors and may +e classified +ys$ape and position, cracks are classed as planar
-
8/16/2019 Weld Defect & Repair,Ham
5/40
Process CracksProcess Cracks
&ydrogen induced cold cracking
(&ICC)
Solidification cracking (&ot #earing)
Lamellar tearing
-
8/16/2019 Weld Defect & Repair,Ham
6/40
CracksCracks
Longitudinal parent metal crack
Longitudinal *eld metal crack Lamellar tearing
#rans%erse *eld metal crack
-
8/16/2019 Weld Defect & Repair,Ham
7/40Transverse crack Longitudinal crack
-
8/16/2019 Weld Defect & Repair,Ham
8/40
InclusionsInclusions
-
8/16/2019 Weld Defect & Repair,Ham
9/40
Gas CavitiesGas Cavities
Root piping
Cluster porosityGas pore
"lo* $ole
&erring+one porosity
Loss of gas s$ield
Damp electrodes
Contamination
'rc lengt$ too large
Damaged electrode flu.
Moisture on parent material
elding current too lo*
Gas pore
-
8/16/2019 Weld Defect & Repair,Ham
10/40
Root pipingRoot piping
PorosityPorosity
Gas CavitiesGas Cavities
-
8/16/2019 Weld Defect & Repair,Ham
11/40
Cluster porosity Herring bone porositySection Ref 3 Shaffie Saad
-
8/16/2019 Weld Defect & Repair,Ham
12/40
!olid Inclusions!olid Inclusions
Slag originates from *elding
flu.
M'G and #IG *elding
process produce silicainclusions
Slag is caused +y
inade0uate cleaning
1t$er inclusions include
tungsten and copper
inclusions from t$e #IG and
M'G *elding process
Slag inclusions are defined as a non-metallic inclusion
caused by some welding process
Slag inclusions
arallel slag lines Lack of interun
fusion 2 slag
Lack of side*allfusion *it$
associated slag
-
8/16/2019 Weld Defect & Repair,Ham
13/40
Elongated slag linesInterpass slag inclusions
-
8/16/2019 Weld Defect & Repair,Ham
14/40
"ack of #usion"ack of #usion
-
8/16/2019 Weld Defect & Repair,Ham
15/40
!urface and profile Defects!urface and profile Defects
Incomplete filled groo%e
2 Lack of side*all fusion
1
2
3 Lack of side*all fusion
4 Lack of inter-run fusion
oor *elder skill
Incorrect electrode
manipulation
'rc +lo*
Incorrect *elding
current/%oltage
Incorrect tra%el speed
Incorrect inter-run cleaning
-
8/16/2019 Weld Defect & Repair,Ham
16/40
$verlap$verlap An imperfection at the toe or root of a weld caused by
metal flowing on to the surface of the parent metalwithout fusing to it
Contamination
Slo* tra%el speed
Incorrect *elding tec$ni0ue
Current too lo*
-
8/16/2019 Weld Defect & Repair,Ham
17/40
Toe OverlapToe OverlapFillet weldFillet weld
Toe OverlapToe Overlaputt weldutt weld
$verlap$verlap
-
8/16/2019 Weld Defect & Repair,Ham
18/40
%oot Defects%oot Defects
Incomplete root fusion
Incomplete root penetration
Lo* 'mps/%olts
Large Root face
Small Root Gap
!ast #ra%el Speed
Incorrect 5lectrode 'ngle
Contamination
'rc +lo*
-
8/16/2019 Weld Defect & Repair,Ham
19/40
Lack o! root !usion Lack o! root Penetration
%oot Defects%oot Defects
-
8/16/2019 Weld Defect & Repair,Ham
20/40
-
8/16/2019 Weld Defect & Repair,Ham
21/40
!urface and Profile!urface and Profile
-
8/16/2019 Weld Defect & Repair,Ham
22/40
Incomplete filled groo%e oor cap profile
5.cessi%e cap $eig$t
Profile DefectsProfile Defects
Poor cap profiles and
e&cessive cap reinforcements
ma' lead to stressconcentration points at the
weld toes and will also
contri(ute to overall poor toe
(lend
-
8/16/2019 Weld Defect & Repair,Ham
23/40
Inco"plete !illed grooveE#cess cap rein!orce"ent
-
8/16/2019 Weld Defect & Repair,Ham
24/40
Profile DefectsProfile Defects
Poor stop$starts
-
8/16/2019 Weld Defect & Repair,Ham
25/40
%patter
5.cessi%e current
Damp electrodes
Contamination
Incorrect *ire feed speed
*$en *elding *it$ t$e M'G
*elding process
'rc +lo*
)iscellaneous Defects)iscellaneous Defects
-
8/16/2019 Weld Defect & Repair,Ham
26/40
)iscellaneous Defects)iscellaneous Defects
'ccidental striking of t$e arc
onto t$e parent material
!aulty electrode $older
oor ca+le insulation
oor return lead clamping
&rc strike
-
8/16/2019 Weld Defect & Repair,Ham
27/40
*ndercut*ndercut
An irregular groove at the toe of a weld run in the
parent metal 5.cessi%e amps/%olts
5.cessi%e tra%el speed
Incorrect electrode angle
5.cessi%e *ea%ing
Incorrect *elding tec$ni0ue
5lectrode too large
-
8/16/2019 Weld Defect & Repair,Ham
28/40
Cap *ndercutCap *ndercut
Measured in +ot$ Lengt$ 6 Dept$Measured in +ot$ Lengt$ 6 Dept$
-
8/16/2019 Weld Defect & Repair,Ham
29/40
Cap undercutRoot undercut
-
8/16/2019 Weld Defect & Repair,Ham
30/40
S$rinkage groo%e
!hrinka+e Groove!hrinka+e Groove
Insufficient *eld metal
deposited in t$e root pass
#oo fast a cooling rate during
t$e application of t$e root
+ead pass
oor *elding tec$ni0ue
A shallow groove caused by contraction in the weld
metal along each side of the penetration bead
-
8/16/2019 Weld Defect & Repair,Ham
31/40
Conca%e root
Concave %ootConcave %oot
Root faces too large
Root gap too large
5.cessi%e +ack purge pressure
during #IG *elding
5.cessi%e root +ead grinding
+efore t$e application of t$e
second pass
A shallow groove, which may occur in the root of a butt weld
-
8/16/2019 Weld Defect & Repair,Ham
32/40
Concave %ootConcave %oot
-
8/16/2019 Weld Defect & Repair,Ham
33/40
-
8/16/2019 Weld Defect & Repair,Ham
34/40
,&cessive %oot Penetration,&cessive %oot Penetration
-
8/16/2019 Weld Defect & Repair,Ham
35/40
Concave root E#cessive root penetration
-
8/16/2019 Weld Defect & Repair,Ham
36/40
Burn -hrou+hBurn -hrou+h
&ig$ 'mps/%olts
Small Root face
Large Root Gap
Slo* #ra%el Speed"urn t$roug$
A localized collapse of the weld pool due to excessive
penetration resulting in a hole in the root run
-
8/16/2019 Weld Defect & Repair,Ham
37/40
urn t'roug'
urn
T'roug'
Burn -hrou+hBurn -hrou+h
-
8/16/2019 Weld Defect & Repair,Ham
38/40
%oot Cokin+$&idi/ed %oot%oot Cokin+$&idi/ed %oot
Loss or insufficient +ack
purging gas
Most commonly occurs
*$en *elding stainlesssteels
urging gases include
argon, $elium and
occasionally nitrogen
-
8/16/2019 Weld Defect & Repair,Ham
39/40
Crater pipeCrater pipe
Weld crater Weld crater
Crater PipeCrater Pipe
-
8/16/2019 Weld Defect & Repair,Ham
40/40
Crater PipeCrater Pipe
Crater pipe is a shrinkage defect and not a gas defect, it
has the appearance of a gas pore in the weld crater
#oo fast a cooling rate
Deo.idiation
reactions and li0uid to
solid %olume c$ange
Contamination
Crater cracksCrater cracks
(%tar cracks)(%tar cracks)
Crater pipeCrater pipe