flow effects on corrosion of steels in...
TRANSCRIPT
![Page 1: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/1.jpg)
FLOW EFFECTS ON CORROSION OF STEELS IN FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT REACTOR PRIMARY COOLANT ––
EXPERIENCE AND UNDERSTANDINGEXPERIENCE AND UNDERSTANDING
Presented at a meeting of the Atomic Energy Society of Japan, ToPresented at a meeting of the Atomic Energy Society of Japan, Tokyo kyo 2008 October 202008 October 20thth
by
Derek H. ListerDerek H. Lister
Research Chair in Nuclear EngineeringDepartment of Chemical Engineering
University of New Brunswick, Fredericton, NB Canada E3B 5A3
![Page 2: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/2.jpg)
2
▲CANDU reactors1. Bruce A
Bruce B 2. Pickering A
Pickering B3. Darlington
■Uranium mines1. Cluff Lake2. McClean Lake3. Midwest
4. Gentilly-1 (decom.)Gentilly-2
5. Point Lepreau6. NPD (decom.)
4. Cigar Lake5. McArthur River6. Key Lake7. Rabbit Lake
● Research reactors1. U of Alberta2. Saskatchewan Research Council3. AECL Whiteshell Labs (decom.)4. McMaster U5. U of Toronto (decom.)6. Royal Military College7. AECL Chalk River Laboratories8. MDS Nordion (decom.)9. Ecole Polytechnique10. Dalhousie U
Fredericton
![Page 3: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/3.jpg)
3
FREDERICTONFREDERICTON
![Page 4: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/4.jpg)
4
UNBUNB
![Page 5: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/5.jpg)
5
NUCLEAR POWER IN CANADANUCLEAR POWER IN CANADA
• In 2007, nuclear ≡ 14.6% of Canada’s electricity• Installed nuclear gross capacity in 2008 (all CANDUs):
OntarioPickering A 4×542 MW(e) (two in safe storage)Pickering B 4×540 MW(e)Darlington 4×934 MW(e)Bruce A 4×805 MW(e) (two being refurbished) Bruce B 1×845 MW(e)
3×872 MW(e)Québec
Gentilly-2 1×675 MW(e) (to be refurbished 2011)New Brunswick
Point Lepreau 1×680 MW(e) (being refurbished)
![Page 6: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/6.jpg)
6
PROSPECTS FOR NEW BUILD IN CANADAPROSPECTS FOR NEW BUILD IN CANADA
OntarioTo decide on technology for two new units in early 2009 (ACR-1000, Areva, Westinghouse)
New BrunswickNegotiating for new unit – Point Lepreau II –ACR-1000 preferred
Alberta and SaskatchewanInterested in new build
![Page 7: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/7.jpg)
7
CANDU REACTORS ABROADCANDU REACTORS ABROAD
Korea (Wolsong) 4×CANDU-6
Argentina (Embalse) 1×CANDU-6
Romania (Cernavoda) 2×CANDU-6
China (Qinshan) 2×CANDU-6
India 3×prototype
Pakistan 1×prototype
![Page 8: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/8.jpg)
8
CANDU REACTOR CIRCANDU REACTOR CIRCUITSCUITS
![Page 9: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/9.jpg)
9
CANDU PHTS CONDITIONSCANDU PHTS CONDITIONS
• D2O with 3-10 cc/kg dissolved D2 (H2 gas added);
• Temperature 265-310°C;
• pH (apparent) 10.2-10.8 (lithium);
• Steam quality at core outlet → 6%;
• Dissolved O2 < 5 ppb (unmeasurable – although coolant may be oxidising at core outlet).
![Page 10: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/10.jpg)
10
MAIN PHTS MATERIALSMAIN PHTS MATERIALS
• Fuel sheaths – Zircaloy 4• Pressure tubes – Zr-2½%Nb• SG tubing (CANDU 6) – Alloy 800• SG heads – carbon steel• Feeders – carbon steel• Headers – carbon steel
![Page 11: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/11.jpg)
11
CANDU REACTOR FACE CANDU REACTOR FACE
![Page 12: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/12.jpg)
12
In 1980s, some CANDUs experienced primary system fouling (reactor inlet temperature rise); e.g. Point Lepreauto May 1989
![Page 13: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/13.jpg)
13
FEEDER THINNINGFEEDER THINNING
In 1996, ultrasonic measurements of wall thickness of carbon-steel outlet feeders at Point Lepreau indicated excessive corrosion: average rates inferred from estimates of initial thickness.
![Page 14: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/14.jpg)
14
THINNING RELATED TO COOLANT FLOW THINNING RELATED TO COOLANT FLOW ––FAC (FLOWFAC (FLOW--ACCELERATED CORROSION)ACCELERATED CORROSION)
FAC α V1.5
![Page 15: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/15.jpg)
15
In 1997, an outlet feeder at Point Lepreau developed a leak – removed and inspected.
Through-wall crack, now thought to be low-temperature creep, possibly exacerbated by hydrogen (deuterium) permeating through metal from FAC.
Several cracked feeders found since – one or two through-wall.
Only at Point Lepreau.
![Page 16: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/16.jpg)
16
INSIDE SURFACE OF CRACKED FEEDERINSIDE SURFACE OF CRACKED FEEDER
• cracks intergranular
• medium-to-high-flow channels
• areas of high residual stress (many tight bends close to reactor face – “warm bent”)
![Page 17: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/17.jpg)
17
ENDEND--FITTINGS AND FEEDERSFITTINGS AND FEEDERS
![Page 18: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/18.jpg)
18
DETAILS OF REMOVED FEEDER INDICATE FACDETAILS OF REMOVED FEEDER INDICATE FAC
Scallops Effects of Cr content of steel
Low-Cr steel a consequence of specifying low-Co material to control activity transport.
![Page 19: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/19.jpg)
19
• All pre-Qinshan CANDUs display FAC: managed by stress analysis, dispositioning, removal and replacement if necessary;
• Darlington plant particularly susceptible (has thinner-wall feeders);
• Following a suggestion and early work at UNB Nuclear and later qualification studies, Darlington injected TiO2 as possible inhibitor into one channel at Unit 3 in 2004 – observed a fall in FAC of > 25%: promising;
• Still too many uncertainties to proceed with Ti;
• Qinshan expected to have low FAC rates because 0.3% Cr steel specified.
![Page 20: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/20.jpg)
20
FAC EXPERIMENTS AT UNBFAC EXPERIMENTS AT UNB
Developed probe for on-line measurement of FAC in high-temperature water loop:
Increase in electrical resistance of thinning tube reflects FAC –“resistance probe”.Probes made from Point Lepreau steel: SA106 Grade B (0.019%Cr)
![Page 21: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/21.jpg)
21
Also developed wire probe – on-line measurement of resistance of thinning wire reflects FAC.
Experiments performed over range of conditions:• flow rate;• pH (LiOH);• [Fe] saturation.
![Page 22: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/22.jpg)
22
These results and plant data suggest shear stress important (flow dependence high).
Scatter of results high …..
![Page 23: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/23.jpg)
23
TENTATIVE CORRELATION DETENTATIVE CORRELATION DERIVED:RIVED:
• Predicts reducing pH from 10.6 to 10.2 will decrease FAC rate by only ~ 12%; differences among plants indicate no consistent trend;
• Predicts flow-rate dependence similar to plant.
N.B. Experiments with coolant nominally saturated in [Fe] still produced FAC – if at a lower rate
CR = 7.65 (1 + 0.111 τ0.75) × (1 + 1.51×10-9 e1.87pH)
![Page 24: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/24.jpg)
24
FAC processes at M-O produce H2
Fe + 2H2O → Fe(OH)2 + 2H ……………(1)
3Fe(OH)2 → Fe3O4 + 2H2O + H2 ………..(2)
Molecular hydrogen from (2) diffuses to bulk coolant.
Atomic hydrogen from (1) effuses quantitatively through metal – measurement reflects FAC.
![Page 25: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/25.jpg)
25
““HYDROGEN EFFUSION PROBEHYDROGEN EFFUSION PROBE”” -- HeProHePro®®
Collection cup clamped to outside of pipe – evacuated periodically –increase in pressure monitored.
Diagram of HePro®mounted on pipe
Typical pressure increase
![Page 26: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/26.jpg)
26
INDUSTRIAL APPLICATIONSINDUSTRIAL APPLICATIONS
Feeder at Point Lepreau
Water wall at Coleson-Cove oil-
fired plant
![Page 27: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/27.jpg)
27
THERMALHYDRAULIC STUDY AT UNBTHERMALHYDRAULIC STUDY AT UNB
• High velocity dependence of FAC suggests shear stress distribution important;
• Full-scale mock-up of feeder and end-fitting constructed from transparent acrylic;
• Mounted in high-flow water circuit, two-phase (air-water) ∆P and phase distribution studied at ~ 25°C;
• Computer simulations with cfd code FLUENT tested against observations.
![Page 28: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/28.jpg)
28Hydraulic loop for testing feeder
FLOW
FLOW
FLOW
FLOW
73o
R= 95.25 mm
1802 mm
ID=54 mm
Flexible Hose
Handle Plug
Air
Spacer
Weir
Sump
Compressor
![Page 29: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/29.jpg)
29
PLANT AND EXPERIMENTAL CONDITIONSPLANT AND EXPERIMENTAL CONDITIONS
CANDU-6 experiment
coolant D2O H2O
temperature (°C) 310 25
chemistry (pH25°C) 10.2 (Li) neutral
voidage 0~0.3 (steam) 0~0.5 (air)
Reliq ~4.3x106 5x105
![Page 30: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/30.jpg)
30
PREDICTABLE FLOW PATTERN IN BPREDICTABLE FLOW PATTERN IN BENDEND
0.05 voidage, Reliq ~ 4.5×105
Flow
![Page 31: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/31.jpg)
31
UNPREDICTABLE FLOWUNPREDICTABLE FLOW PATTERN IN BENDPATTERN IN BEND
0.2 voidage, Reliq ~ 4.2×105
Liquid film
Flow
![Page 32: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/32.jpg)
32
![Page 33: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/33.jpg)
33
FLUENT FAFLUENT FAILS TO PREDICT PHASE ILS TO PREDICT PHASE DISTRIBUTION IN BENDDISTRIBUTION IN BEND
0.2 voidage, Reliq ~ 4.2×105
1.0
0.0
Air
Test section mid-plane
Recirculating flows influenced by upstream end-fitting
![Page 34: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/34.jpg)
34
SCALLOPINGSCALLOPING
• Effect of surface sculpting as “scallops” still unknown;
• Research at UNB Nuclear indicates scallops cannot be treated as conventional “sand-grain roughness” (i.e., influencing ∆P via Moody relations);
• Scallop shapes create different ∆P in forward and reverse flow;
• Experiments under feedwater conditions (FAC at 140°C in neutral water) indicate constant “scallop Reynolds number”.
![Page 35: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/35.jpg)
35
PROCESSES PROCESSES TO BE MODELLEDTO BE MODELLED
![Page 36: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/36.jpg)
36
MMODEL REFLECTS SYNERGY BETWEEN ODEL REFLECTS SYNERGY BETWEEN FILM DISSOLUTION AND SPALLINGFILM DISSOLUTION AND SPALLING
• Electrochemical processes affected by potential – ECP computed in parallel;• Diffusing Fe2+ predicted to be unchanged Fe(OH)2 – straightforward Fick’s
Law applied;• Rate constant for magnetite dissolution from literature (one reference)
SHOULD CONTROL (<<m.t.c.);• Same rate constant assumed for precipitation (no reference);• Erosion treated stochastically – random-number generator used to decide
size of particle to spall from size distribution;• Time for particle to be loosened and removed;
• When particle disappears, film thins instantaneously by d and corrosion rate jumps.
CkQd
di Δ⋅∝τ
θ
![Page 37: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/37.jpg)
37
MODEL PREDICTS (MODEL PREDICTS (using CFD code to calculate using CFD code to calculate local shear stress)local shear stress)
• corrosion rates at different positions in feeders;
• ECP ~ -700 to -900 mV (vs. SHE);
• oxide film thicknesses (0.7 μm to 3 μm);
• growth of oxide to steady-state;
• corrosion and oxide film thickness of inlet feeders (saturated in dissolved iron, lower temperature).
![Page 38: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/38.jpg)
38
PREDICTED OXIDE FILM THICKNESSES IN PREDICTED OXIDE FILM THICKNESSES IN OUTLET FEEDERSOUTLET FEEDERS
![Page 39: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/39.jpg)
39
PREDICTED CORROSION RATE AND OXIDE PREDICTED CORROSION RATE AND OXIDE FILM THICKNESS FOR INLET FEEDER: FILM THICKNESS FOR INLET FEEDER:
![Page 40: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/40.jpg)
40
MODEL FITS PLANT DATA WELLMODEL FITS PLANT DATA WELL
FAC α V1.5
![Page 41: FLOW EFFECTS ON CORROSION OF STEELS IN ...wchem.sakura.ne.jp/wp/wp-content/uploads/2019/09/第5...FLOW EFFECTS ON CORROSION OF STEELS IN REACTOR PRIMARY COOLANT – EXPERIENCE AND](https://reader034.vdocument.in/reader034/viewer/2022042620/5f489cb4a0e1ba43b866b6b0/html5/thumbnails/41.jpg)
41
ACKNOWLEDGEMENTACKNOWLEDGEMENT
Many people at UNB Nuclear, including students passing through and graduating, have contributed to the findings described in this talk; my thanks are due to them.
The Centre for Nuclear Energy Research (CNER) at UNB is thanked for ongoing collaboration.
Finally, I am grateful to the CANDU Owners Group (COG) and its partners and the Natural Science and Engineering Research Council (NSERC) of Canada for continuing support for UNB Nuclear.