Formulation 2K Waterborne PUR based on Bayhydrol A-145/ Desmodur XP 2410 using HALOX SW-111 Formula Constants 10.81 Density (lb/gal) 1295.82 Density (g/L) 23.20 Weight Pigment (%) 8.05 Volume Pigment (%) 69.02 Weight Solids (%) 59.21 Volume Solids (%) 27.43 PVC (%) 0.73 VOC (lb/gal) 87.31 VOC (g/L) Formula Properties pH @ 25°C 8.0 - 8.5 Viscosity Part A- Stormer @ 25°C 80 - 85 KU Pot Life 3 - 4 Hours Supplier Key Bayer Corporation [1] Rohm and Haas [2] BYK - Chemie USA Inc. [3] Lanxess Corporation - Borchers Paint Additives [4] DuPont Chemicals [5] HALOX [6] Ciba Specialty Chemicals [7] Cure Ratio by Wt. (A:B) 3:1 Cure Ratio by Vol (A:B) 2.5:1 GALS LBS COMPONENT A: GRIND 234.69 26.53 Bayhydrol A 145 [1] 54.77 6.56 De-Ionized Water 7.00 0.78 Tamol 681 [2] 1.50 0.17 BYK-028 [3] 1.77 0.20 Borchi Gel LW 44 [4] 228.91 7.03 Ti-Pure R-960 [5] 33.00 1.38 HALOX SW-111 [6] High speed disperse to 7+ NS Hegman grind. 251.50 28.43 Bayhydrol A 145 [1] 4.70 0.56 BYK-346 [3] 1.50 0.17 BYK-028 [3] 4.77 0.52 Tinuvin 5151 [7] 19.81 2.37 De-Ionized Water COMPONENT B: 285.10 29.70 Desmodur XP 2410 [1] 104.41 1,129.02 TOTAL HALOX® 1326 Summer St., Hammond, IN 46320, USA tel: 219.933.1560, www.halox.com A-145 XP2410 SW-111 The information contained herein is correct to the best of our knowledge, but is intended only as a source of information. The recommendations or suggestions herein are made without guarantee of representation as to results, and we suggest that you evaluate the recommendations contained in this formulation in your own laboratory prior to use.

Upload: others

Post on 15-Feb-2021

2 views

Category:

Documents


1 download

TRANSCRIPT

  • Formulation2K Waterborne PUR based on Bayhydrol A-145/ Desmodur XP 2410 using

    HALOX SW-111

    Formula Constants

    10.81Density (lb/gal)

    1295.82Density (g/L)

    23.20Weight Pigment (%)

    8.05Volume Pigment (%)

    69.02Weight Solids (%)

    59.21Volume Solids (%)

    27.43PVC (%)

    0.73VOC (lb/gal)

    87.31VOC (g/L)

    Formula Properties

    pH @ 25°C 8.0 - 8.5

    Viscosity Part A- Stormer

    @ 25°C

    80 - 85 KU

    Pot Life 3 - 4 Hours

    Supplier Key

    Bayer Corporation [1]

    Rohm and Haas [2]

    BYK - Chemie USA Inc. [3]

    Lanxess Corporation - Borchers Paint Additives [4]

    DuPont Chemicals [5]

    HALOX [6]

    Ciba Specialty Chemicals [7]

    Cure Ratio by Wt. (A:B) 3:1

    Cure Ratio by Vol (A:B) 2.5:1

    GALSLBS

    COMPONENT A:

    GRIND

    234.69 26.53Bayhydrol A 145 [1]

    54.77 6.56De-Ionized Water

    7.00 0.78Tamol 681 [2]

    1.50 0.17BYK-028 [3]

    1.77 0.20Borchi Gel LW 44 [4]

    228.91 7.03Ti-Pure R-960 [5]

    33.00 1.38HALOX SW-111 [6]

    High speed disperse to 7+ NS Hegman grind.

    251.50 28.43Bayhydrol A 145 [1]

    4.70 0.56BYK-346 [3]

    1.50 0.17BYK-028 [3]

    4.77 0.52Tinuvin 5151 [7]

    19.81 2.37De-Ionized Water

    COMPONENT B:

    285.10 29.70Desmodur XP 2410 [1]

    104.41 1,129.02TOTAL

    HALOX® 1326 Summer St., Hammond, IN 46320, USA tel: 219.933.1560, www.halox.com

    A-145 XP2410 SW-111

    The information contained herein is correct to the best of our knowledge, but is intended only as a source of information. The

    recommendations or suggestions herein are made without guarantee of representation as to results, and we suggest that you

    evaluate the recommendations contained in this formulation in your own laboratory prior to use.

  • Water Based Polyurethane500 HOURS SALT SPRAY - SUBSTRATE: BLASTED HOT ROLLED STEEL

    80 microns - % on total formula weight

    3% Zinc Based Competitor 3% HALOX SW-111 Corrosion Inhibitora-145xp2410-sw111-e