Page 1: Process problems & trouble shooting in cement kiln

RNB CEMENTS (P) LIMITED DEPARTMENT- PROCESS Presented By- Akshay Kumar Si DGM (Process)05/01/23 1

Page 2: Process problems & trouble shooting in cement kiln

05/01/23 2

Page 3: Process problems & trouble shooting in cement kiln

WHAT ARE THE MAIN PROCESS PROBLEMS IN CEMENT PLANT?In Pyroprocessing- Cyclone Jamming Kiln inlet jamming Big clinker ball formation Coating formation in kiln Feed rushes and dusty kiln Snow man formation in cooler Red river in clinker cooler

05/01/23 3

Page 4: Process problems & trouble shooting in cement kiln

PROCESS PROBLEMS IN GRINDING Mill jamming Residue problems Blaine problems

05/01/23 4

Page 5: Process problems & trouble shooting in cement kiln

Cyclone JammingWhy cyclone jamming happens in Preheater?

Main Reasons-Insufficient suction due to low rpm in PH fan.Flap valve failure & blockage in material pipe.Refractory failure.High Iron % in Raw mix.High Sulfur % in fuel(i.e- coal)

05/01/23 5

Page 6: Process problems & trouble shooting in cement kiln

KILN INLET JAMMINGWhy kiln inlet jamming happens?

Main Reasons- High Iron % in Raw mix. High Sulfur % in fuel(i.e- coal)

05/01/23 6

Page 7: Process problems & trouble shooting in cement kiln

BIG CLINKER BALL FORMATION

Why big size clinker ball formation happens?

Main Reasons-High Iron % in Raw mix.High Sulfur (S)% in fuel(i.e- coal).Kiln running with slow rpm & % filling is more.High BZ temperature.% liquid is more.Higher % of Magnesia (MgO).

05/01/23 7

Page 8: Process problems & trouble shooting in cement kiln

HEAVY COATING FORMATION IN KILNWhy heavy coating formation in kiln?

Main Reasons- High Iron % in Raw mix. High Sulfur (S)% in fuel(i.e- coal). Kiln running with slow rpm & % filling is more. % liquid is more. Higher % of Magnesia (MgO).

05/01/23 8

Page 9: Process problems & trouble shooting in cement kiln

FEED RUSHES & DUST KILN

05/01/23 9

Why Feed rushes and dust kiln happens?Main Reasons- High lime in Raw mix or high LSF.Very less % of liquid.High AR.Less iron% in raw mix.Blockage of hot meal due to clinker ball

occasionally.

Page 10: Process problems & trouble shooting in cement kiln

SNOWMAN FORMATION IN COOLER

05/01/23 10

Why snowman is formed in cooler?Main reasons-Higher % of liquid, may be iron % is more in

raw mix so hot meal will be sticky and viscous.Shorter cooling zone; so may be shortage of

adequate quenching .Higher BZ temperature, may be due to short

flame.Failure of air blaster in cooler 1st grate if any.

Page 11: Process problems & trouble shooting in cement kiln

RED RIVER IN COOLER

05/01/23 11

Why red river is shown in cooler?Main reasons-Uneven distribution of cooling air.Mis alignment of kiln & cooler.

Page 12: Process problems & trouble shooting in cement kiln

RED RIVER

05/01/23 12

Page 13: Process problems & trouble shooting in cement kiln

THANK YOU