![Page 1: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/1.jpg)
*'^W0p^/m>ffv**i.[} "J" •• .'j,wmmfm}f^^f^. 'imäif$^m3>mwfy^,m*f^.^ww^
AD-758 754
Stress Corrosion Cracking and Hydrogen Embrittlement of High-Strength Fasteners
Aerospace Corp.
APRIL 1973
Distributed By:
National Technical Information Service U. S. DEPARTMENT OF COMMERCE
- ■ -■■-"■-!- .^--^ ,.;...-...,,tJ.J........ ., ...: -... .,.......,
![Page 2: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/2.jpg)
,,,
THIS DOCUMENT IS BEST QUALITY AVAILABLE. THE COPY
FURNISHED TO DTIC CONTAINED
A SIGNIFICANT NUMBER OF
PAGES WHICH DO NOT
REPRODUCE LEGIBLYo
![Page 3: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/3.jpg)
»'^a^^isj^iiw^ffisffP'?^^'^^.^ -v.
AIR FORCE REPORT NO SAMSO-TR-73-131
AEROSPACE REPORT NO I R-0073(341 301) - 1
Stress Corrosion Cracking and Hydrogen Embriltlement of
H igh-Slrenglh Fasteners
I'up.ucd IM I K >l AM I 'S
M .i [ i i" i .i N SM t in t s I IIMU i(iit •,
I .1 111 11 .Hill \ () I'd .it mi ■-
. APR sO
Ss si t tils I ni; i in i I i ii L: ( )pi ■ .i I I i' I. \
HI A! ROSPAC I ( ORPOR A I ION
•• D D C
[ 'A APR It b.. I'
B
Prepared tor SPAM AM) MISSILI sV^IIMS ORCiAM/ATluN
AIR i:{)R( I SV.STIMS ( OMMAM)
LOS AM,! US AIR I()R( I STATION
Ins .Atiics. ( i! i; < • t ii i .i
APPROVED FOR PUBLIC RELtAVf D IS T R i B Ü T l O N UNLIMITED
![Page 4: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/4.jpg)
fwMMW"*-—, . .;Wff,.»-Min^^*-r »*f^sw'^*^^^<r~««ft^f,}.
LABORATORY OPERATIONS
The Laboratory Operations of The Aerospace Corporation is conducting
experimental and theoretical investigations necessary for the evaluation and
application of scientific advances to new military concepts and systems. Ver-
satility and flexibility have been developed (o a high degree by the laboratory
personnel in dealing with the many problems encountered in the nation's rapidly
developing space and musile systems. Expertioe in the latest scientific devel-
opments is vital to the accomplishment of tasks related to these problems. The
laboratories that contribute to this research are;
Aerodynamics and Propulsion Research Laboratory: Launch and reentry aerodynamics, heat transfer, reentry physics, propulsion, high-temperature chemistry and chemical kinetics, structural mechanics, flight dynamics, atmo- spheric pollution, and high-power gas lasers.
Electronics Research Laboratory: Generation, transmission, detection, and processing of electromagnetic radiation in the terrestrial and space envi- ronments, with emphasis on the millimeter-wave, infrared, and visible portions of the spectrum; design and fabrication of antennas, comp'.ex optical systems and photol.'thographic solid-state devices; test and development of practical superconducting detectors and laser devices and technology, including high- power lasers, atmospheric pollution, and biomedical problems.
Materials Sciences Laboratory: Development of new materials; metal matrix composites and new forms of carbon; test and evaluation of graphite and ceramics in reentry; spacecraft materials and components in radiation and high-vacuum environments; application of fracture mechanics to stress corrosion and fatigue-induced fractures in structural metals; effect of nature of material surfaces on lubrication, photosensitization, and catalytic reaction«, and development of prosthesis devices.
Plasma Research Laboratory; Reentry physics and nuclear weapons effects; the interaction of antennas with reentry plasma sheaths, experimenta- tion with thermonuclear plasmas; the generation and propagation of plasmn waves in the magnetosphere; chemical reactions ot vibrationally -sxciud species in rocket plumes; and high-precision .sser ranging.
Space Physics Laboratory; Aeronomy, density and composition of the atmosphere at all altitudes; atmospheric rrai tiou" anu atmospheric optics; pollution of the environment; the sun, earth's resources; mot;orological mea- surements, radiation belts and cosmic rays, and the effects <->f niclear explo- sions, magnetic storms, and solar radiation on the atmoi >cic
THE AEROSPACE CORPORATION El Segundo, California
m;u,'
\-
r ;ts
......-..,-■..-..- **....** : . ■
:..--.-.:
![Page 5: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/5.jpg)
Air Force Report No. SAMSO-TR-7 3-131 Aerospace Report Nu.
TR-0073(3413-01)-1
STRESS CORROSION CRACKING AND HYDROGEN
EMBRITTLEMENT OF HIGH-STRENGTH
FASTENERS
Prepared by
.1. K. Stanley- Materials Sciences Laboratory
Laboratory Operations
73 APR 30
Systems Engineering Operations THE AEROSPACE CORPORATION
Prepared for
SPACE AND MISSILE SYSTEMS ORGANI7A PIOiV AIR FORCE SYSTEMS COMMAND
LOS ANGELES AIR FORCE STATION Los Angeles, California
Approved for public release; distribution unlimited.
- ■-- ■ ■-•—-'■■-.■■-•-■- ■■-^^-.■.■. .-^ ^ v. . ,.ii :^..- -;:Uj,t .... .^t.. ...^-aL^^aAk.Ui ..Vl*f«^^,VA-»#5*=i^*«»yMM^-i-^v?v.V.-'>-
![Page 6: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/6.jpg)
IHiPfPPIilPliPiPPpii;
FOREWORD
This report is published by The Aerospace Corporation, El Segundo,
California, under Air Force Contract No. F04701-72-C-0073.
This report, which documents research carried out from June 1971
to January 197Z, was submitted on 11 November 1972 to Colonel Frank B,
Alford, Jr., LVCA, for review and approval.
Approved
Mft W. C. Riley, director Materials Scvences Laboratory Laboratory Operations
S. 'Lafäzan, Group Director Titan III Directorate / Veiiicle Systems Divisiqn Systems Engineering Operations
Publicatinn of this report does not constitute Air Force approval of
the report's findings or c> nciusions. It is published < nly for the exchange
and stinuil.ition of ide.iis.
J^faii**& & Frank B. Alford, Jr.^ Col. , USAF Director, Titan Engineering and
Test Space Launch Vehicles SPO
-ii-
*.^-,r;,-wir^a*wpa.M.*-« r*±,kr**±~*M***.*-*' W^ T ■- I •■-^■;—"" ""'^
![Page 7: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/7.jpg)
PfPppBSPpssssptSW!
S<-( unl V • I.ISSJI Ji .U ion
ÜOCUMENT CONTROL DATA - R 8. D Security c tas itltc allon ol Utlo. hotly ot abstrnct ami indexing «nmWfl(/on niu.sf he ttntertid when th« overott feptttt (.*. < lumtltlctt)
1 ORIGINATING ACTIVITY (Corporatö authur)
The Aerospace Curporation El Segundo, California
i ti REPORT SECURITY CLASSIFICATION
Unclasoified 2 ft GROUP
3 RCPORT TITLE
Stress Corrosion Cracking and Hydrogen EmbriUlement of High-Strength Fasteners
4 DESCRIPTIVE NorE5(TVp»o( report and Inctuatve date»)
5 Au THORISI fF/r«r mm«, mtddla Inltlcl, Imal . a)
James K. Stanley
6 REPO RT DATE
73 APR 30 8/1 CONTRACT OR GRANT NO
F04701-72-C-0073 h PROJEC T NO
7o TOTAL NO OF PACES
49 7b NO OFREF5
39 9^1 ORIGINATOR'S RETPOHT NUMBER'S;
TR-0073(3413-01)-1
SAMSO-TH-7-.-131
10 DISTRIBUTION STATEMENT
Approved for public release; distribution unlimited.
II SUPPLEMENTARY NOTES 12 SPONSORING MILITARY ACTI
Space and Missile Systems Organization Air Force Systems Command United States Air Force
13 ABSTRACT
Unexpected, brittle failures of high-strength fasteners on aerospace vehicles have been caused by stress corrosion cracking (SCC) and by hydrogen stress cracking (HSC). Despite extensive study, much remains to be learned about the phenomena. The poorly understood failure mechanisms are difficult to differ- entiate, especially in the field. There is a growing .-.se of the term SCC to describe failures by both mechanisms.
Data are given to characterize the classes. For low alloy carbon steels heat- treated to yield strengths below ~160 ksi, stress corrosion is not a problem, nor is hydrogen embrittlement (delayed cracking) very common. Above 160 ksi, difficulties can occur. The high-strength, precipitation-hardening, stain- less steels have varying degrees of resistance to stress-corrosion cracking and hydrogen embrittlement, depending upon strength level and heat-treating pro- cedures that influence the microstructure.
Consideration of plane strain fracture toughness K^Q and stress corrosion threshold Kjcrr; parameters allows selection of optimum bolting materials for a specific environment. The advantage of plane strain fracture toughness analysis is that it does not differentiate between failure mechanisms; failure can be by either SCC or HSC.
DD F0RM '473 4 ACS M . , t imQLAl
^ccuniv ( l.i ss ;'n .ii i^n
aftwim^miftrmmWMiiihi^ n^m^Mn^vu^m^^r^rru-- -„■^^^,..u^..^^^- ;.^^.J.^^^.,^-.^.:.. .. ..||,
![Page 8: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/8.jpg)
^mm^^^mmmmm^im^m^m^w^^w^^^^^^^^^^ ^mm^w!^fi!:'^^^^Wf!^W'^!W^
UNCLASSIFIED Set un i\ < LihMÜi .itmii
KEY WORDS
Bolt failures Brittle fracture Fracture mechanisms in bolt selection High-strength fasteners Hydrogen embrittlement Stress corrosion cracking
Distribution Statement (Continued)
Abstract (Continued)
y i' UNCLASSIFIED ^ Security Classititation
OtfM -'—-"—"^-'^- ^-im-i irni ■ i iirniiiwriiliiriiitiiiB-|iii^^ SSM -.-.^^.^^^-^^^^^.
![Page 9: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/9.jpg)
ilBP^Pl"^ PfWVW**.^)?!
CONTENTS
FOREWORD ii
ABSTRACT iii
I. INTRODUCTION 1
II. DEFINITION AND DIFFERENTIATION OF STRESS CORROSION CRACKING AND HYDROGEN STRESS CRACKING 5
III. MATERIALS FOR HIGH-STRENGTH FASTENERS . . . .13
A. Classifiralion by Strength Level M
B. Classification by Campositiun and Metallurgical Structure 14
C. MartensiLic Steels 17
D. Stainless Steels (Austenitic and Ferritic) 17
E. Precipitation-Hardening Stainless Steels 19
F. Superalloys (Nickel-Base and Cobalt-Base) 20
G. Classification by Relative Resistance to SCC .... 20
IV. FAILURES DUE TO SCC OR HSC ON THE TITAN III FAMILY OF VEHICLES 2^
V. THE PROMISE OF FRACTURE TOUGHNESS CRITERIA 27
VI. RECOMMENDATIONS <1
A. Prevention of SCC and HSC 57
B, Data Collection and Test Standardization i:<
VII. CONCLUSIONS >)
REFERENCES 41
-v-
i-.ii,.L-lu.ii-'i]HTilir:'-X-..:'ir-i i-ilii1-i;iriiiitfit>i—irT—"—■''-'■''—^■'^■1-*^^'^-1 ' n'^flMliav , -, jciMrt/mli-t. .fr,/,^.^-,^^..-.,^^^^^^^^«^^.^«^^«!!»!^^^«*»-
![Page 10: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/10.jpg)
wmm*ß^>^ßMß^m^w®V'm^ ■* amamKX-^Jm mmmmn WBPBIB
TABLES
2.
3.
4.
5.
6.
Nominal Compositions of All Alloys Mentioned in the Text 8
Differences in Failures by HSC and SCC 10
Materials Highly Resistant to SCC Z2
Materials Highly Resistant to SCC if Used with Caution 23
Materials with Low Resistance to SCC 24
Fastener Failures on the Titan III Family of Vehicles 26
Fracture Toughness Rating of Alloys and Heat Treatments for Resistance to Saltwater Environments (Northrop Data) 34
Fracture Toughness Rating of Alloys and Heat Treatments for Resistance to Saltwater Environments (Boeing Data) 35
Results of Sustained-Load Experiments with Notched Specimens of Various Ultra-High- Strength Steels Exposed to a 5% Salt-Fog Atmosphere 36
-VI-
fei^il^A>te'^*»J^^■^:^'^^^^M[^^TB^^l^rtfll■^^i ;HAh,;^WUl.«-,^*U^&TCMI^W-) I .>i^^wV^a^-W^''-4l^''*UrWW:~^^:'-tr ---'.l T.-f i^J^irt'rFr^lC
![Page 11: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/11.jpg)
*=»>ML.(wm ™******mmmimm**m mWwmmw^m
FIGURES
1. Delayed Failure Characteristics of 4340 Steel at Various Strength Levels Resulting from Exposure to Distilled Water at 68 F 7
2. Typical Data Obtained from Potentiostatic Tests 12
3. Classification of Low Alloy Steels (Martensitic Types) by Strength Range 15
4. Classification of Stainless Steels and Superalloys by Strength Range 16
5. Typical Behavior of a High-Strength Steel in a Corrosive Environment Zr)
6. Delayed Fracture Characteristics of 4340 Steel at Various Strength Levels Resulting from Exposure to Distilled Water 30
7. Data of Figure 6 Normalized by Use of the Stress Intensity Ratio 31
-vii-
'—•■-"'-■-■■---—-'•- "-----"-•-"■-"■'tm^^^^
![Page 12: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/12.jpg)
ißjßm^WM'M'ßWfM&W ■■IPIPBiPHWIIHIPW fmsmmwvwm-iiw^'Wm W' 'Ti'"" '-"'T'«1
I. INTRODUCTION
The design engineer may not always be fully aware of Lhe possibility
of brittle failures in fastener systems that could result from stress corrosion
cracking (SCC ) or hydrogen stress cracking (HSC ). The failure of high-strength
fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently
and almost always unexpectedly. There is a growing acceptance of the term SCC
to co\er both mechanisms. The term 'environmental stress cracking1 failures
is also used sometimes.
Perhaps some of the reasons for occasional surprises from these phenom-
ena are that (1) the existing knowledge v.as no* available to the designer, (Z) the
possible ha/.ard was recognized but ignored, (i) the existing knowledge was not
believed applicable to the current situation, and (4) there was insufficient test-
ing on a new material before it was commercialized. Designers should not de-
sign fasteners by handbook only. There are no reliable handbooks for material
selection for possibly ha/.ardous situations.
Very few fastener failures can be attributed to deficiencies in the technol-
ogy of high-strength materials. Part of the difficulty can be traced to inadequate
dissemination or utilization of available information and i '■ the unrealistic assess
ments of technology by the improperly informed, failures generally occur from
inadequate knowledge of environmental conditions.
Any systems as sophisticated as those in aerospace application should use
a fastener system to realize the full benefit of high-strength fasteners. A sys-
tem requires proper material selection for bolt, washer, and nut. ikolt heads
(hexagonal or IZ-po'nt), boll-head fillets, and radii at base of threads are all
important aspects of good bolt design. Cart? should be exercised in selection
of nuts and washers. The use of uashers produces more uniform loads. Nuts,
if not properly selected, can fail by SCC or HSC.
HSC refers to hydrogen embrittlemenl, hydrogen cracking, and hydrogen induced delayed cracking.
-1
rnrrMl~'-:i-^"'^"i"'"iaa"»"B'
"n iH^rtif-1'
![Page 13: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/13.jpg)
W!IWi5?S|!PE|gfPWWWS5?H^ -T^r^iP^wm:—!^mTW^!*^rit-i>i' ■. ' .M-li \\l*ll_Hßiimi: ■ .^•:--'J"l'"u* '*- * -lft.lf>\
l.illli- allention is preäetitly given to torque - tensicn relationships in fas-
tener systi-nih, althouuh ari appreciation of this relationship is essential to opti-
mum structural design, since the function of a fastener sy /turn is to furnish a
clamping; lorce or load, Oplimum design requires torquinji that will capitali/.e
on the full strength potential of the bolt. Use of preload indicating devices and
strain gages is often necessary, so that the loa.ds placed on a bolt are known.
Many engineers have no idea of the clamping forces in their structures, Effects
ol contact surface finish on components, coatings (if any), lubrication, asym-
metrical holes, and torquing anrl retorquing on the same boll are frequently not
appreciated. When 70 to 80 percent of the energy of torquing is expended in
overcoming friction on a dry bolt-nut combination, little energy is available
to develop a clamping force.
Fatigue of the fasteners in aerospace hardware has not been a problem,
ma:nly because acceptance testing time and flight times have been too short
(less than 1 hr) to develop failures with the stress loadings. However, on the
space shuttle that aims for 100 flights, fatigue (jf fasteners could become a prob-
lem. As parts subjected to higher stress are used, more attention must be
given to steel cleanliness (inclusions act as crack nuclei), to radiuserl threads
(to .-educe notch effect), and to larger head shank fillets (also to reduce notch
effect). High-strength fasteners should have threads and head shank fillets rolled
on after heat treatment, and shanks should be ground anrl polished. Rolling
threads after heat treatment builds up a residual stress to counttract a portion
of the applied tensile load, and it ensures unbroken grain flow lines through the
critical area created by the notch effect of the threads. Hood (Ref. 1) reports
experiments in which the threads and !"illets were rolled before and after heat
treatment. The 260 ksi (UTS) bolt rolled before heat treatment had a time to
failure in SCC of 2 hr, whereas if the threads and fillets uere rolled after heat
treatment, the bolt had a time to failure of 74 hr.
The incidence of fastener failure has been decreasing because engineers
have learned to avoid materials that have given difficulties in the past. Solutions
are not always as simple as a material substitution, but may be complex, involv-
ing material changes, use of coatings, redesign, or reduction of stress, or a
-2-
ttvmimmmmmimiammiMim jliifiaiiaMiiimiiMiM
![Page 14: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/14.jpg)
PTOtWiHiiiiiii#u,-.,.iiJ,J ^.--■i^.mS'MWM^u^.,- wmmmm pywJU^UJJiiiJJLviuifiuii IU(MI111UJ1U,IJ,111^
cumbinaiion ul thesu ( Kel . ^ I. i he re a n-, ui cou r s<;, many (J1 he r I \ l)^■ .^ • i. 1.»■-
lener failures, L'.U., uve rt<; rqumji and stri;ris r.pti.rt-, but l.iilui'cs i.-- .1 ri'biilt
of stress-cor rosiun or hyflrogen enii;rill ICIIUMII .1 :■'■ most itibif.'ious.
E^erause ul a lack ol standa rdi/e'l le.sl ii.i-iho'l'- :or S('.(. .ind lor li~<-, sta-
tistical analyses ul data arc not feasible. A.S'J.M is aiii^i-i', v. ori-inu in iini . irca
to develop standa rrli/"d tests lor both phenomena."
As the st re njit 11 level ine reases ai)o\ e ~ 1 t.D k s 1, liot h the sens it 1 v 11 •. I 1 l)r il
lie fracture and the suseeplibilily lo SCC and ii.S(^ IIK ri'.ise. Althoai;!". •-t.i-l-
with st rengths in excess of 3 00 k s i ire aval 1 able, desi une r s a re !•■ 1 ' 1 ' to
push for this strength level and have settled on levels of ^00 to JnO ksi. .^ume
designers who have experienced either SCC or M.SC ha\ e even nickel •'.': '
strengths of 160 lo 180 ksi.
SCC and HSC have caused many serious and nne \ pec; e<. lailures m iiudi-
st-ength fasteners. Failures 'ia\ e occtirreri in .ippl ical luiis at slresses thai
appeared safe (below the yield strengthl 1 rom stress malvses, even with the
use of generous factors of safety. These failures have led designers '" use
materials far below their true capabilities, either by ustrit; less than optimum
strengths of a high- strength steel or by using steels heat -1 reated to the maxi-
mum strength at very low strenqth levels, say .' • uercenl ul the vu id strenulh,
Hoth SCC and HSC^ involve chennc il end n a.-t d hi ru 11 1! laitors tliat are
poorly understood. Much research ha been 'loin.' in various en-. 1 roi 'i.enl s lo
establish relative sensitivity ol mate n 1: s lo these 1 v> u n.ei h snisius. Media ri re
often chosen to give accelerated failure. Metallurgical slruci r. s have been
studied extensively so that crack initiation and propagalion ■• .in ije l-eller
understood. So far, this approach has not been parlicularlv : ••,. ';..l.
Some of the difficulty in understanding thi tvo fracture modes arises
because they are so much alike. Hydrogen appears to be '.he cuipnl in both
phenomena. It is only in the laboratory, by electrochemical means, that the
'The American Society for Testing and Materials is seeking to develop test procedures in the areas of stress lorrosioi. cracking and corrosioi :ati<4ue smooth test specimens, environments and materials, precrack uriv.l.h, sub critical crack growth, and hydrogen embrittlement.
• 3-
BttttiftiEtoiistfit ViÄ<e!#«iifiäÄ4i8fiy lll^iWiriTIMillfllliniiliiilWlWiiililMWWili'llM if 1^
![Page 15: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/15.jpg)
mmnß^mm**) iininunmnuJuu-^-ii .■■ .L..II.JI.U^.-t!--^,j.j|.j-,-j-.1-. .—-. 1 wep!PW!W^tU!4l,P-t'' !■.' iim^-i.^-Jmujiui
'v.n 11 u-e hamsnih can be uniquely differentiated. In the field, it is difficult, il
nut impussibic , to identity which cracking phenomenon was responsible for the
tailurc. St ress-corrosion theory is not sufficiently advanced to predict failure
limes. There is a need for a unifying theoretical mechanism for explanation
ol SCC and 1ISC.
However, despite many similarities, the basic mechanisms are differ-
ent. Although brittle failure in high-si rength steels exposed to aqueous envi-
ronments has been well documented, there is still controversy concerning the
mechanisms ol delayed failure. Relerence i contains a useful discussion ol
Hi- :. K-t hanisms of failure m SCC.
Shotpeening, plating, and painting of low alloy, high - st rength martensitu
laslcncrs as a means of preventing delayed tailures at ambient temperatures
has been largely unsatisfactory. Current interest lies in use of HSC- or SCC-
resistant stainless types and superalloys (nickel-base and cobalt-base).
Whuch of these two mechanisms is responsible for failure of a metal fas-
tener is generally of academic interest to the engineer. Because HSC and SCC
are so similar, the same type of solution will often suffice for both problems.
-A.
Aa^^i^^:;^-'....- ....■.^^^,.^.^.^tK:-^^ih^^li^i.^^.,^ M&ssitSäliäälS&iliiäl^^
![Page 16: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/16.jpg)
mmmimmmmmmf^ im^mMmmmMmaf. tmmiMiuik-mmM^iirii'k1^1**'^-!'*1-^
II. DKl'lMIIO.X AND DII'KI-;KK;\ Tl ATIO.\ Ul' HTKLSS CORROSION
CRACKING AM) H i'hKOCiKA S.'RIiSS ClACKINCi
Excellent reviews of SCC and HSC arc to In- lound in Rets. 4 and ->.
Stress corrosion cracking is nucleation of a crack in a susrcptiblc metal
in a corrosive environment while the metal is stressed in tension: the crack
then propagates by stress - inrluced cor rosion of the arivancing crack, tip. Crack-
ing may occur inte rgranularly or t ransgranuiarly, depending on the metal
and its heat treatment, failure occurs v,ith little or no plastic deformation,
the fractures are termed brittle failures. The stresses are generally below
the yield stress.
The SCC occurs in specific environments and with environmentally sen-
sitive metals. In most cases, there is negligible loss of metal by general cor-
rosion, and at times the corrosion is imperceptible to the eye. Stress corro-
sion cracking requires highly anodic areas and a locali/.ed pll, such as may
exist in oxide film cracks, pits, crevices, and cold-worked areas.
HSC occurs because ■J hydrogen penetration into the lattice ui the pres-
ence of a tensile stress. It is generally agreed that corrosion plays no direct
role in this mechanism. However, corrosion often plays an indirect role as
the source of hydrogen.
In classic HSC, the hydrogen is introduced into solid solution by electro-
lytic charging, pickling, heat treatment, and corro:-ion reactions. Hydrogen
then causes delayed failure under static load in high-strength alloys, and the
embrittling effect increases with increase in severity of notch, i.e., stress
concentration (Refs. 6 and 7). Tests for HSC have not been slanna rdized; ihe\
should include both machine - not ched and precracked specimens.
Obviously, if no hydrogen is present in the lattice, no HSC can ocmr. if
hydrogen has entered during pickling, heat treating, or electroplating and is
removed by baking in air or vacuum, no HSC will occur when tensile stresses
are applied. The amount of hydrogen that will cause HSC is exceeding]^, small,
of the order of 4 or 5 ppm. Damage has been reported with hydrogen contents
..,:..,..-, ..::i^M^Ü fijaUBMÜÜttÜÜi immämmaMiimmm \
![Page 17: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/17.jpg)
mrnmrnm***'!" ÜM M- WWfWW.i UUUV, I ■lä^gWMiMWii.Di m^',. H
üi i'\en Ifss than I ppm (Rcl. -1). The v.ork oS Ma/.ancc and Sc-jnoha iRel. H)
HULim'sts that (tclayed traclurcs in as-Cjiicni hid sleula ^rc due* lo some pr<jper-
t u's öl ihc martensile transformation it.icli and not to hyfl rtjgcn, Delects in the
auslfiiili' gram boundary occur as a result ol dynainu eltt.'Cls caused by grov -
niL ii )a rl ens 111' plates. Thesu delects an1 a source ol weakness in the prior nus-
trnitc gr.iin boundaries and give rise to delayed liailurc.
The delayed lailure characteristics ol '1340 steel, which «vas exposed to
distillefl water anri failed presumably by 11SC, are shown in Figure 1. (Xonn-
nal compositions of all alloys mentioned in this report are given in Table 1.)
Similar failure characteristics are caused by SCC. Note in figure 1 the short
time to failure of the 4340 as the ultimate tensile strength (UTS) ol the steel
increases and the threshold stresses below which no lailure occurs (Ref. 7).
The important parameters in these delayed failures are strength levels,
steel composition and metallurgical structure (microstructure), tensile stresses,
environment (i.e., tendency toward corrosion or introduction of hydrogen), and
time. Increases in temperature seem to increase the likelihood of SCC more
than thai of IISC, the latter occurs around room lempe ral ure. The tensile stresses
can be applied stresses, residual stresses (as in roll-formed threads, heat
treatment, welding, straightening, or cold-rolling), or a sum of these stresses.
If residual stresses are present, they are very difficult to measure or estimate
so that one does not know their magnitudes. For either SCC or HSC, there
exists a threshold limit below which the stresses will not cause fracture.
In the laboratory, the electrochemical behavior of the metal offers per-
haps the best arguments that SSC and HSC are separate, distinct phenomena.
Delayed cracking that occurs under cathodic polarization (hydrogen polarization)
can hardly be attributed to SCC, Conversely, delayed fracturing where anodic
polarization is causing dissolution (cor rosion) of the metal can hardly be identi-
fied as HSC. The polarization vs time to failure curves identify the two mech-
anisms uniquely. Obviously, such methods would have limited field use. Brown
(Ref. 9) and Bhatt and Phelps (Ref. 10) have proposed this type of electrochem-
ical procedure for distinguishing between SCC and HSC. SCC occurs by defi-
nition when cracking involves corrosion at anodic areas of the advancing tip
-6-
&üaiiiitA«J^t£)*
^^^mp^m^^immmmmmimmmmmmmmLn ^ tiiriiiiirim
![Page 18: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/18.jpg)
11. --I.U-J.^.4;JJ-^1- llll!|IJjl.lll|ll 1 ,!l.,-Ll.m.!IWJ^)k4l>....-J- t-W-^'J1'1'»'^'.-!" ■■Jyi^^«lJ:I^PWlliP.m"WttllUll.l.iPJinillJM!piuiJj||ljj ... = |U LutLUJIM- ■ i JJ ■-
240
200
0 —
\ 10"
TEMPERED AT 800CF TO A 205ksi STRENGTH LEVEL
TEMPERED AT 400oF TO A 285ksi STRENGTH LEVEL
10 I02
TIME TO FAILURE, mm I05 ;o4
Figure 1. Delayed Failure Characteristics of 4340 Steel at Various Strength Levels Resulting from Exposure tu
Distilled Water at 68 F (Ref. 7)
-7-
.,:.^ ■....-,.;.,/,:..^.,.,.-^,..-J1^,.^...:;.^.it.w4-..aa.,,»^^^^ ...■„.U,.'..,.-^.;„,.-:i \t^aira;|-.;.w^,.a.;i ■■■ i , , -. ■■!■ -;. ...- -..-■ ::■:-.■.:■.■.. ....::,■.
![Page 19: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/19.jpg)
^■U-.UUiUjjg^ifgWl^ll|WW«-iW!llW!li'M#|i ',- i1 !JJ-.ai;j|^HgpjWHWMipw.^^MWiaw*>^.Mii...i i!iüi»if^^^ju,i|..J-..»jp-u^BW.^-i^^1,.'i^-'^»M*'-*-4^^^^,^^ IIMIJIJI iiminiijijj.i . M
I alile 1. Nominal Compositions of ALI Alloys Mentioned in the Text
1 I
-1 !
- ■ - ----- — -'— 1 ,
', il
M-, A in i . Al "Hi.. j
i'. 2.
4 Mu ■ 1 1.4I
4 1-»' - 1 :.1 1.1' 1...1
" ' 1 1 t.-il '•.^■■
in 11 1 . - • 1 -1 '. .1 ' ) . -l ! 1 t . 1 .Sj [
:K \. ■'.V I , DD 1,41 1 . ' n. ■!; \ |
in ■ t ".1 1 . -■ ■ •<. 1 " -1
1 -.
. HI i,ji
1 .
'- ' ( . 0. in
M.. r .»■' . ii. .1 • IH , , . ■ 1..1 4.H.II 11,-11, u. 1 'i j
v-'' "'■ "''
t v|.. !(■ . 1 '■■
1,.,
1 , •' ■ '
i * ,■■ i:: 1 ' II. h i,..i l.i.n 1. ,. ". .■ ■ \ ■
i s... -t i 1 ' i'. 1 • 1 < 1. - i M,. u. i I.I" i; i,.il ". ■
ii 11 11,-11 i 1. .1 1 . »H i. ■ V
1 .' 4 I'll
i; ■ rii i, .i .
ii
1 7 UH
■1. Il li.il 11. t
l.ll)
I'll 1 . Mr. II. in 1- II 1 ~. 1 h.ll 2 . ', 1 1. VII
I'll 1 1-N Mu II. n-, 1.' 7 ■> H.I' ll.ll .' . 2 .
1 I'll 1 1 - M.,
1 ^ ■ I'M
n.io
ii. U7
M
11
1 i h . 1
-1.
l,..l
l.dl
. . ',11
II. t
1.111
AM ii. 1 ,. It, 1. •> I...I 2. '( n. 1 ,N
AM > .-. il. 1J 1 •1. -i l,..l 2. ■• '). 1 N [
An .■ n.iil 1-1 i.. IMI II.Ml
In, „,,-l 7IH o. n ■, 1 ■> 11 2i,, 11 bal 1 .2i 2.1-. '). J 1). 1 \
Mj>ri.-»-:i o. i II in n In. ( 1 -> . 11
il <.ll' , Wl III
l.i stun. -1 -i n.n-, 1 1 -,-, li.il 11. S 11. > I.I J. ii C.u
A J.ii i). (i-. 11 7., li,il 1 . 1 2. 1 1 t). t S 0. ) v 1
Ml' l-.N Jn 11 1-, , V . tl 1 H. 11
II.1.-.1. Il.n X i). in H (1 l,.il 1 IH. ', '." U.i,
Kin. -11 ii.n t il 11 li.il 11 .11 1 11. 11 1. 1 1 •', W.,s|, .(„v II. 117 1 ' IMI It 2. 11 ■1. 1 2. '. (1.7
.m iin.-l X7 '.(1 ". IM 1 ', l.,.l 7.11 II.''^ 2.S 0.7
lyp,- 111 ll. 1 • Ih 0 '/. li ll.ll
1 VP'- KM 11. 1IH 1 1 s '*, '. IJ.II
lyp.' im 11. ill 2 i (1 1 1. H ll.ll
lypi- Ut, II. OH 17 (1 '2.11 I1..1 2.2-,
i yp.- m a. ab IH 0 1 l.ll lul bxc
Typ.- I-47 1). UH IK 11 1 1 .(1 l.,.l ioxr 1 nit. nip J 1 J il. OK 1 n 0 I'y.u li.il CI.SO 4.0 0.1^
iMM*jAiti^ia^^teVHV^-^a,ate-4taäaa^
![Page 20: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/20.jpg)
WWj!!!W,.a».. 4 mMMm,W< IMWJL ■ ■■uti'.."' —-' tj^iuiiJ ..iy.in...iiij|i üt^iJiJMt^..J BP'.'!JI*!»Ml."S-MJ^ip-»*ll
(Kcl. I I ). I1SC t)\ (lc 11 ml ion is i ru 1; i .'ifj ni'lu' IM| by hydrogen ^ern-iatjun ,il
the 11 [5 l)\' icitho'ln i u r rcnl s , I )il I c ri-nvcs lli.it li.ivc Itct n (.cnr ral I y noted in
lailurrs dur to IlSCi or S('(' ,ii'c (jiwti in I'.ihli- .! .
Many tost proo'durus are USIMJ to evaluati- suscuptiljility to SCCand lISCl.
A common SCC It'sl to establish susi-eptibil ily ol ijar slock involves loading the
specimen to some high percentage ol it'.i vielt] stress, or sometimes UTS, and
exposing it to alternate immersion in a 3. i percent XaCl solution lor ! (J mm
and drying in forced air :or 50 mm. The cycling is continued until the speci-
men fails or the test is discontinued. The sodium chloride is usually dissolved
in distilled water or is acidified (to pll of ~l.5). Imposed stresses generally
vary from 75 to l*() percent of the tensile strength of fatigue-c racked notched
specimens and from T-> to 90 percent of the ".2 percent yield strengths of un-
notched specimens.
Austenitic steels are commonly checker] for SCC by exposure to -4 2 per-
cent boiling aqueous MgCI^ (I54C, JO'M') solution; lerritic stainless steels, by
contrast, are relatively immune to cracking in MgCl ,> (lief. 12).
Until recently, SCC tests were conducted on smooth specimens. These
tests are helpful in selection of materials for environments or in development
of coatings. They could not be used, however, lor establishing safe design
loads. Often there is large scatter in the data. The SCC tests on both smooth
and precracked specimens used in fracture toughness studies provide the designer
with tools for material selection on the basis of service environments that
can be simulated in the laboratory. The testing methods, however, need
standardization.
For the HSC test to establish susceptibility, a notched specimen is loaded
to 75 percent or more of its notched yield strength, and hydrogen is cathodi-
cally charged into the steel vhile it is under load. Sometimes a notched speci-
men is plated with electrolytic cadmium and then loaded. A notched specimen
is more susceptible to HSC than an unnotched one. Cathodically charging a
steel with hydrogen provides considerably more hydrogen than is necessary to
produce a delayed failure. Loadings are similar to those used for SCC tests.
■9-
••;i>ii-l--;',-'uV^"'^t:'" ., . itimimmmmmm^mmmmmmmmmmmmtmmmjmmm^ — ~~^-~~~^
![Page 21: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/21.jpg)
able Z. 1 )il iC rt'iv.L'S iri [■"diluresj by 1ISC atvl SCC
use SCC
Rupture nucleation inside the Rupture nucleation at the metal- |
metal or at notches environment interface originating
from pits
Single crack v>.ith minimal Extensive branching and several
branching secondary cracks j
Electron microscopy may show No striations are observable on
strialions indicative of Hiscon- the fracture face 1
tinuous (.rack propagation. (Do
i not conlu.se v. itli latiguc
striations.)
Presence of flat dimples and Flat dimples and hairlines on
hairline lattices on the grains, grains are less numerous than in
as seen by electron microscopy HSC, as seen by electron |
microscopy j
No corrosion is ordinarily Corrosion products are evident
present by microscopy
Occurs mainly in martensitic Occurs in many alloys (ferritic,
steels at very high ultimate austenitic, martensitic) over a
j strength levels wide range of UTS levels
-10-
ljlltgMMBaMMttlBlMttBali^^
![Page 22: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/22.jpg)
ip^^yujrJM^MW.^^^
High-strength bolts must also pass a si rcss-durability (static fatiguu)
lest. The bolls are slresseci lo 1 ^ percent ol Ihe Piininium t( nsile load .nd
are held lor 46 hr. Il eniliriltied by hyflrogen, they will fail.
The potenliotlatic proceriure is becoming more popular lor the study ol
both SCC and HSt'. Figure I shows that IS-HPII steel can be made to lail by
either phenomenoil if the potential is changed (Rel. 13). This type ol test can
probably be standardized to assess the relative susceptibility of a given steel
in various heat-treated conditions to either SCC or HSC. The lest is definitely
a laboratory tool and would yield guidelines rather than design data.
In environmental cracking failures at the launch ranges, it is not possible
to unequivocally separate HSC from SCC. Therefore, the failures are often
attributed lo (1) stress - cor rosion cracking (v.hich includes SCC and HSC) or
(2) environmental stress cracking. For engineering purposes, this may be
sufficient. Pinpointing the actual failure mech-.nism may be ol academic inter-
est only .
Fleet ron I ractography with the transmission electron microscope or the
newer scanning electron microscope cannot uniquely identify HSC. Flectron
microscopy is a very useful tool when used in conjunction with other tools. A
knowledge of circumstances leading to failure is a valuable adjunct to success-
ful failure analyses. The compilations of electron fractographs by AFMI. are
helpful in deciding what the nature of the failure mode may be (Ref. 14).
Intergranular and cransgranular cracking result from hydrogen, a suscep-
tible microstructure, the specimen geometry, and static or dynamic tensile
loading. It is not true that intergranular cracking is typical ol SCC and that.
transgranular cracking is characteristic of HSC. A review (Ref. 15) of 3'*
studies involving fractography of materials failed by HSC and SCC found ZZ
instances of fully or predominantly intergranular cracks, 8 instances of fully
or predominantly transgranular cracks, and 8 mixed cases. Intergranular crack
ing appears to be the most frequent type in both HSC and SCC.
11
■,..:-..■.,.;.. ■.. ..!.:■! ■-' ^x--:-:.::!^:^,i.\^I.:i..:L:{..^::. i&iiitiisi^'. ^^i^Hi^iSi'M^t ̂.„..^^^u^..*:^^,.^^ ^iiUUiM^^ IHMMiaMMMiifittJüiAiia&daiiaMsaaMfliiii ViiiWihiMWiiWitt^^
![Page 23: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/23.jpg)
iBHP ii&i^wiwmm&jmivwi***1!™?'?* i^^WW!!tfP^''IW^IIJ-1JPU'"IM''1'|'lti?M-'j
Ul Q O
o
J UJ Sr O _J <r
Q QL <I
CO
CO
o
12"
08
UJ \— o CL
04
0
-04
-08
I 2
16
20
TESTS CONDUCTED w[ 31/2% NaCi LOADED TO 0 9 OF NOTCHED UTS
ANODIC CONDITION (METAL DISSOLUTION)
7-4PH AGED , , lhr900F(H-900)
I7-4PH AGED Ihr 950F(H-950)
CATH0DIC CONDITION HYDROGEN GENERATED
10 I02 I03
TIME TO FAILURE, mm
10^
Figure Z. Typical Data Obtained from Potentiostatic Tests (Ref. 13)
12-
u-xM--.«cimfntirwiftifr»nTi ''' I'HWTW
![Page 24: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/24.jpg)
Ill JJ^IMI'llMIPMIipipilll»!!' ■JM-A»-!» »J5?™i>Jii|iswu<l-«.ni,i|-,«*<:,j.'':'" ;gppW^^B(.j«MjmtiPLii|jJMU»wyjJU4P.^^HJiJ!!:fl''lfH'>^wH^^^
III. MATERIALS FOR illi;il Si Ul.NCi ASTL'NKRS
The ncrosparc industry has i-mphasizcd Ihr systnas corn rpt uf lasten»-»
for Ihr saki- ol reliability. Desijjn has been improved so that btrnnger, lijjhti
and more sophisticated fastener systems are available. Environmentally resi
tant fasteners have recently been stutlii'd.
Steel composition is important, as is the metallurgical structure. Ihc
time for initiation of the first crack in either HSC or SCC depends on the
mic rest rue tu re resistance to hydrogen diffusion or pit corrosion.
Much is known empirically about what compositions and structures arc
susceptible to HSC or SCC, but little is known from first principles about the
relation of mic rost ructure to crack initiation and propagation. Most data are
basically phenomenological. Tiner and Galpin (Reference 16) are among the
few to attempt studies of mic roprocesses involved in SCC.
Nuts and washers must also be carefully selected for the fastener sys-
tem. Careful selection means that the nuts are also subjected to a SCC test,
generally torqued on a bolt and submerged in salt water. Washers are used
to distribute the load. They too should be compatible with the bolts so that
they do not produce galvanic corrosion. Because they are loaded in compres-
sion, they do not fail by HSC or SCC.
Materials for aerospace fasteners are categorized in several ways:
(1) by strength levels, (2) by composition and metallographic structure, and
(3) by relative susceptibility to SCC and HSC. In the future, the steels will
be categorized by fracture toughness parameters; some such compilations
are already appearing ano are discussed in Section V.
A. CLASSIFICATION BY STRENGTH LEVEL
One arbitrary classification of threaded fasteners is by ultimate str* ngth
range:
low strength
medium strength
< 125 ksi
125-160 ksi
-13.
- ....'..■ ^::..:l:ii- T- ,■-■,, nr ->^---•,> ^ ■-^ Vi. ■ I- r..^v.^-..V^V.w-t^..-;.Jv<^r;^ -„.. im m am aas^flsa
![Page 25: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/25.jpg)
h i L;1I st rcntith
ult ra-hiuh st rciTM h
1H0-260 ksi
• Z « 0 ksi
i iuur( 5 ahovvs the strength ranges fur some popular alloy steel
fasteners. Fmure 4 shows the strength ranges lor some stainless steels
and superallnys.
Of course, stri-nglh luveis disclose neitfier the type, composition,
and mir rost ruclu re of the materials nor susceptibility to SCC anrl HSC
B. ("LASSIFICATION BY COMPOSITION AND METALLURGICAL
STRUCTURL
Another classification, by type of alloy, is useful to the understanding
of the behavior of these materials; alloys are
ma rtensit ic,
stainless steels (austenitic and ferritic),
precipitation-iia rdening stainless steels ( semi-austenitic '.nd martensitic), or
superalloys (nickel-base and cobalt-base)
Experience has shown that some types of high-st rength steels art.' quite
susceptible to SCC and HSC while others are not. Some change in degree of
susceptibility to SCC results from the precipitation of grain boundary carbides
and the presence of secondary phases. Corrosion theory is not sophisticated
enough to explain this phenomenon.
Steels used at or above 160 ksi UTS should meet AMS-2300A cleanli-
ness standards. Steels should be vacuum- or consumable arc-melted for
minimization of inclusions, which can cause pitting. Mechanical properties
sometimes can be higher and more uniform with greater toughness if steels
are vacuum melted.
•14-
.;....,-.„,.^..f, gaBgjaaaaeieMaiBiMaftBBiiaBiMMMiMi .it.-..!.;..^.,-,. ■- ■■■■■ I -....■■■la.lili.r.lrriill-li'iWr.i«- -■■ .■.«*!>*■.■■'- •■"'^■■•■^■■^C-U-AUi.
![Page 26: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/26.jpg)
**z*™^*im'!mTt.T**"?',','r'''*''~'=''''~'J' y" ■ ■■ir'f'"-vMi-.-f"-'f7. i„,.a.iit-.;:L_w..jji<tfBjfe).!i,i,t.w IH:<J
ALLOY r"rrL5
STRCNGTH RANGL
ULTIMATE TLN5UF STRENGTH, ksi
i MEDIUM r* IÜÜ 150
-HIGH 200
-^[JLTRA-HIGH, 250 300
4130
4140
4340
8740
HY-TUF
D6AC
H-ll
HP9-4
MARAGING-200
MARAGING-250
MARAGING-300
□
I I
Figure 3. Classification of Low Alloy Steels (Martensitic Types) by Strength Range
(The wide ranges of strength of some of the steels are ob- tained by tempering at different temperatures. )
-15-
jjjayli^.s.».»;....,■.... , ^.,--..,.■■ ».^„i;i^i.-L,%-^.^,:-..v.aw:i^^^^
![Page 27: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/27.jpg)
■^^■^■Mj'iy.lwi,iiiii!W|.^Hij|. ^w.;lMl^^M.vu!^Vll';°-■ YJ^W»'"^1''/1^.^ -r-nTs-'-r- ■Tg-j":?—--ix-r f-v!.-r--
STAiNLESS STEELS AND
STRENGTH RANGE ULTIMATE TENSILE STRENGTH, ksi
MEDIUM h- HIGH SUPERALLOYS ioo 150 200
-1 ULTRA-HIGH 250 300
TYPr 410
TYPE 416
TYPE 422
TYPE 431
I7-4PH
I7-7PH
PHI5-7Mo
PHI3-bMo
PHI4-8M0
I5-5PH
AM 355
INCONEL 718
HÄYNES-25 □ GUSTOM 455
1 l l
i 1 _ . ^
A286 i ;
MP35N HASTELLOY-X
RENE -41 i i
WASPALOY 1 1
Figure 4. Classification of Stainless Steels and Superalloys by Strength Range
(Dashed lines indicate strengths obtainable by cold-work and aging. )
16-
.,,v-...:. .■.^.. c..-/;:-..-^-^^;,^^.!^^.-^^^ ■ , i,.,.,,,.,.,^...,.., , ..|8M,--.w^,.^-^
![Page 28: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/28.jpg)
rVT^V vw^^^^^p^^wtmm^r^^^J-Mf^i-iL^^ * ''jgVK y?f:i*rr,'&*Q
C. MARTENSITIC STEE_LS
For carbon and low alloy steels heat-treated to strength levels of
< 160 ksi, SCC is not a problem nor is 1ISC common. In the martensitic
steels, there is a ductile-to-brittle transition raniZ'.;, and crack growth
takes place differently above and below the range. Above the transition,
envii onmcntally induced slow crack growth occurs over a large area before
catastrophic failure occurs. Below the transition, significantly less crack
growth is observed before total failure occurs. Below the transition, a
martensitic steel has poor impact or impact-tension properties. Fasteners
made of 11 - 1 ' steel heat-treated to -w 2 00 ksi are usable to -65° F before the
transition is reached.
The austenit ic-type stainless steiVs and nickel-base alloys (Inconel
7IH, Waspaloy, AZH6, and MP ^N) have no such transition and actually
have enhancer! mechanical properties at cryjgenic temperatures.
In martensitic steels, the prior austcnite grain boundaries appear to
facilitate hydrogen diffusion. It is probably true that all martensitic steels
will fail by IISC under severe conditions. Retained austenite facilitates sus-
ceptibility to SCC (Ref, 17).
The maraging steels can develop strengths > 300,000 psi; thus far they
have had limited application at this level, but at lower strengths they are
usable alloys. These steels are cooled from the austenitizing temperature
to form a soft and weak martensite, which is hardened and strengthened by
aging a! S50-(l^0°F. The fracture toughness of these materials is good up
to yield strengths of -^ZSO ksi.
D. STAINLFSS STEELS (AUSTFNITIC AND FERRITIC)
The austenitic steels of the Type 300 series are much loo weak" to be
considered for use in high-strength fasteners. Only through cold work and
MIL Handbook 5A assigns Types 301, 302, 303, 304, 316, 321, and M7 yield strengths of 30 ksi and ultimate tensile strengths of 75 ksi.
-17
MBaäiJMkiaaafaaayBa^MgMäMttaia ^^wi-ji^iry^.Mi'itn^'.i.wj-^t.^ L-^^:^.^.^.../.'-/..^^-.^^:...!*^^.:^ ■.■-■■-::..•:■/^
![Page 29: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/29.jpg)
^■jMm^'HJV-;,:|»'j-''''",'-w^
stress relief can high strengths be developed in these materials; half-hard
materials have a UTS of 150 ksi, while fully hard materials have a UTS of
185 ksi.
Even though the annealed materials have low strength levels, the alloys
can be fractured in environments containing chlorides. Suss (Ref. 17) reports
SCC failures with stresses as low as 2000 psi in an environment of 50 ppm
sodium chloride. The annealed materials are very resistant to HSC. Pitting
on these steels can occur at emergent sli- lines as well as at inclusions.
Precipitation-hardened austenitic r ?kel chromium is also available.
Alloy AZH6, one of the first, is now one of the most popular high-strength
stainless steels. If the alloy is cold-worked (60%) and aged (1200oF),
strengths > 200 ksi are attainable. Alloy A286 has outstanding resistance
to SCC and HSC. In potentiostatic experiments at The Aerospace Corp.
Material Sciences Laboratory, it has been impossible to fracture the alloy
under anodic or cathodic conditions. Field experience confirms the alloy's
high resistance to these phenomena.
Ferrite in an austenitic steel (Type 304) retards SCC that may have
originated in the austenite. Type 301, when cold-worked over 20%, shows
marked susceptibility to HSC because of the martensite formed from the
austenite by cold work (Ref. 12). Stainless steels containing a mixture of
austenite and martensite may fail by either HSC or SCC, depending on the
environment. Additions of silicon to austenitic steels in concentrations i 5
percent arc claimed to make the steels immune to SCC (Ref. 18).
The ferritic stainless steels. Type 400 (e. g. , 410, 416, 420, 422, and
431), are heat-treatable to strengths of ^200 ksi. Although these steels are
martensitic in structure, they are not generally considered in the martensitic
class because they have relatively high chromium contents, ^-13 percent.
These types have good general corrosion resistance but they are suscepti-
ble to SCC. This susceptibility can be removed by tempering at 1100°F or
higher, but high strength is sacrificed (Ref. 19). Reference 20 recommends
limiting the use of 13 percent chromium in corrosive service to ^140 ksi.
■18-
fca».^.,-.^i:....v,..,^^u.^;^ -.r,.-..>,o.^vJi...^.m.,.<v,,a^^^^^^ g riTiMlMJi
![Page 30: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/30.jpg)
Piipippipppippipiipllpffi ^psppgH^^^ipraps^JWisssrrBB^^
Failure üf the ferritic stainless steels by SCC is intergranular or
transgranular, depending on the tempering temperature (Refs. ?A and 22).
When cracking is intergranular, the fracture follows the prior austenite
grain boundaries (Ref. 16). The high susceptibility to cracking in the prior
austenite grain boundary is ascribed to the presence of c-carbide. Delta fer-
rite, sometimes present in Type 410, increases susceptibility to SCC (Ref. 17).
The 13 percent chromium martensitic stainless steels, when tempered
in their secondary hardening range, have minimum resistance to SCC or HSC
(Ref. 23). Phelps and Loginow (Ref. 24) have shown that a 13 percent chro-
mium steel, when tempered above 900° F, has a minimum time to failure in
the Kure (N. Carolina) Beach atmosphere.
E. PRECIPITATION-HARDENING STAINLESS STEELS
The precipitation-hardening stainless steels offer high-st rength,
unplated, corrosion-resi stant alloys that can resist: HSC and SCC, which have
been experienced with plated and unplated martensitic, low-- and high-alloy
steels in the range from 200 to 250 ksi.
These precipitation-hardening steels have varying degrees of resistance
to SCC and KSC depending, of course, on strength level but also on the tem-
perature of the aging treatment. Aging below 1000° F may make these steels
susceptible to SCC and HSC, but aging above this temperature makes them
very resistant to these cracking phenomena. The reasons for this behavior
are not well understood.
The precipitation-hardening steels are of LWO basic classes, marten-
sitic and semi-austenitic. The martensitic types are 17-4 P1I, 15-5 PH,
and PH 13-8 Mo. In these alloys, the martensitic structure forms upon cool-
ing from a solution treatment; subsequent aging between 900 and 1 150ok
strengthens the martensite by precipitation hardening and tempering. Typi-
cal semi-austenitic steels are 17-7 PH, PH 15-7 Mo, PH 14-8 Mo, and
AM 350. • In these alleys, the composition has been adjusted so that the
■i9'
tew^jaAiaa^i^MMiäi^^ ££»
![Page 31: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/31.jpg)
SS^PP^P^SI?!<Sf«jHai»Ä»?JW«W Wlfl!Ki^(^sp«M!5«^!'|!??w??,^T" TTW^m^m^^^
austenite forms upon solution treatment and is retained at room temperature.
In this condition it is readily fabricated (cold-worked). The hardening is
obtained by reheating the austenite to 1400 or 1750° F (called conditioning),
cooling, and finally aging at 950 or 1050oF.
If either of these steels is overaged beyond highest strength, both the
fracture toughness and the SCC resistance are improved.
The fracture toughness and SCC resistance of martensitic steels are
significantly higher than those of the semi-austenitic types, probably because
of the absence of delta ferritic and grain-boundary carlndes (Ref. 25).
F. SUPERALLOYS (NICKEL-BASE AND COBALT-BASE)
In general, the greater the nickel content in the austenitic steels, the
greater their resistance to SCC and to HSC.
Ultra-high-strength stainless fasteners are madd from superalloys
(high-strength nickel-base and cobalt-base alloys). The nickel-base Inco
718 superalloy, cold-worked and precipitation-hardened, has strengths in
excess of 200, 000 psi.
The new and highly alloyed MP-35N exhibits the corrosion resistance
of the best nickel-base alloys. It is highly resistant to SCC and to HSC in
salt environments and marine atmospheres. It is a fairly new material,
and little experience with it has been obtained.
G. CLASSIFICATION BY RELATIVE RESISTANCE TO SCC
A third classification (Ref. 26) rates materials according to relative
susceptibility to SCC and can be used as a rough guide to material selec-
tion based on experience and some laboratory work. This classification
comprises (1) alloys and heat treatments that can be used without restric-
tion, (2) alloys and heat treatments that must be used with caution, and
(3) alloys and heat treatments that should not be used.
-20-
-iliiiiLHi JJt- ^BA^ik; llgllllllljgjgll ■~ti ti ■:--'.-^i---'.-^i i /i-^Jrt -uj^^-re. M ^■n,^,,^^^,^^ -.,.. .....,^^,..i..-.^j;..a-..;::.„..- ^.....^...^
![Page 32: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/32.jpg)
««"«Ä^^W^^W'-r^W^'W^^
These materials are clescriljetl in Tables 3-5. The tables apply only
to SCC in environments of sodium chloride solutions, salt sprays, alternate
immersion (wetting and drying), and marine atmospheres. Similar tables
for HSC are not available.
These ratings are not to be construed as exact, because no attempt
has been made to evaluate the effects of stress, environment, metallo-
graphic structure, and time. These tables represent the type of SCC data
that was available before the advent of fracture mechanics. No attempt has
been made here to incorporate data obtained by fracture mechanics and given
elsewhere. Other factors of concern to the aerospace materials engineer
are the metal-propcllanl compatibilities, which are not discussed here.
-21-
(■Afe-l^Sii^fe^.iffiijajiiaiiiiii^^ Jmht:r-;„»-t-:—\-'./ Wi—i.v;ftfIJ'.'i-l/fe;.;riiliin-r ,-»■ i— - ■ .f rii ■■i-i i--.-lii V-nmiiMruW'n-f I■ri'"'.
![Page 33: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/33.jpg)
^Mvw$$£$^$i!$iwzn^*??^^ i i,t*i*-*Jw**^&y^Y-^\3JFSVZ^^ Iff^gQg^glB^^msSM^SBm^'SfSft/m^i^n^i mm I fwm^fT'?*?» ■ -l-..-^.,,..,^-.,.^.--.-. wHWiyiw*gBfiM|i
Table 3. Material« lli^hly Resistant to SCC
M.lt ITl.ll^ Type Heat Treatment3 Remarks j
^00 scrii-s stain- less types 303, 3 04, 316, 32 1. 3-17
A u s'. e n i 11 c Annealing Stressed material can crack in chloride solutions. Annealed mate- rials are not of high strength. | Cold-worked materials can develop high strength but they must be j st ress- relieved. |
17-4 PH Martensit if H 1000 and above
17-7 PH Semi-austenit u CM (100 Strength is developed by cold- working (60%) and aping ((100oF).
Pll 13-K Mo M a r t e n s i 11 e H 1000 and above
l^.S PH Ma n ensil n MIOOO ami above
PH IS-7 Mo Si-nii - .unitemt n rn loo Strength is developed by told- \ working (60";,) ai.d agmp (,*00UF).
PH |4.H Mn S.-MII .uisremt it CM oOO Same is pll 1 ^.-7 Mr..
AM ^0 S<-iiii .uisr.-ml ii S( TI00O ami above
; AM l1^ Semi - aus! eint 11 SCTI000 and above
Cv]stiiin-4Sci Semi-a\ist enit ic HI 000 and above
A 2H6 Austenitic Solut ion-treated and a^ed
A 28b (CW and Aged)
Austenit ic High strength is developed by cold- working (60%) and aging ( UOO^F).
Inconel 7lH Face-centered cubic
Solution-treated and aged
Inconel X-7S0 Face-centered cubic
Solution-treated and aged
Rene-41 Face-centered cubic
Solution-treated and aped
MP 3CN Face-centered cubic
S<»lution-t reated and aged
Solut ion-annealed, cold-worked 60%, and aged.
V'aspaloy Face-centered Solut ion-1 reated
and aped
Low Alloy Steels 4 1 SO. 4 140, 4 340. S74Ü
Martensitic Quenched and tempered
High resistance to .SCC if tempered to 1 60 k si or lower.
Ma raping Steel Ma rtensitic Solution-treated and aped
High resistance if heat-treated to 200 ksi or lower.
For heat treatments, refer to Aerospace or steel producer's literature.
Structural Metals Handbook, Metals Handbook ASM.
-22-
■ ■"^' --- ^-..v... ■"■ vmm-i,iiriri ...„.v.:.^^!^^-...^^.^.-^.-^^
![Page 34: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/34.jpg)
?w<Mß^w*&wm'.*w&&7^' ** 'iwsmsairaffWHi n '/^''-T1^! :^^rr^^'»*5T7K37^T-'^^»(7Tipr?r*.^T'l BSI w^i^3^;^'3TT?i^Kr™',-~i-r?-i'-i;pi^?'=^*»iTr:i^T'iTr''P,TT-vr" wn
Table 4. Materials Highly Resistant to SCC if Used with Caution
Materials Type Heat Treatment Remarks |
Low-alloy steels 4130, 4140, 4340, 8740, D6AC, HY-TUF
Martensitic Quenched and tempered
Good resistance to SCC if tempered to ■v 160- 180 ksi
Maraging steel Martensitic Solution-treated and aged
Ma raging-200 and -250
400 series stain- less 410, 416, 422, 431
Martensitic Quenched and tempered
Not susceptible if tempered at 1 100° F or higher
15-5 PH Ma rtensitic H?50 to H1000
PH 13-8 Mo Martensit ic 119 50 to HI 000
17-4 PH Martensitic H950 to H1000
AM 355 Semi- austenitic
SCT 950 to H1000
-23-
.-;^w^w..^v.^^^ik^-^;^^.t<^uM^^ ■—— ; ^— ■■'- ■■■■•■-■■-■-
![Page 35: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/35.jpg)
-'*'^t^^T^^r^:-ri--rT^T^rrf^^^ 'i^fzwrvm" rv Tr^ry-n .-Tj-,.,..^.,,7-,^<,T._-ll„,^I...,J_,>,_lv...„.,. ,.| ^.,^^,t.
Table 5. Materials with Low Resistance to SCC
Materials Type Heal Treatment Remarks |
Low- alloy si eel s Marl ensit ie Quenched and Very susceptible to 41 -.O, 4 140, tempered SCC if tempered to 4340, 8740, 1H0 ksi and higher | D6AC, HY-TUF
Ma raging Martensitic Solution-treated and aged
Maraging-300
H-ll Martensitic Quenched and tempered
17-7 PH Semi- All heat- austenitic treatments
except CH900
PH 15-7 Mo Semi- All heat- austenitic treatments
except CH900
AM 355 S e m i - Heat-treatments austonitic below SCT ft00
400 series stain- Martensitic Quenched ant) Very susceptible in less 410, 416, tempi; red the secondary hard- 4ZZ. 431 ening range from 500
to 1000oF 1
-24-
— :----.nN,1Y»^»i«MVi..iiWWIW^riMfa^^
![Page 36: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/36.jpg)
^4paww|is»impw'^
IV. FAILURES DUE TO SCC Oll HSC ON THE TITAN III FAMILY OF VEHICLES
The Air Force Titan III Frogram has had difficulties with high-strength
fasteners on the boosters during the past 6 or 7 years. Table 6 lists some
of the fastener steels and modes of failure. Failures were all in a marine
atmosphere. The precipitation-hardening steels have all been slowly
replaced by the cold-worked type of A286. The 440C and H-ll were continued
in service, but either their heat treatments were modified or protection by
organic coatings became a requirement, or both. Type 212 was eliminated,
but Type 431 was continued in service with organic coatings; long-range
solutions involved substitution of A286.
These failures occurred during the early years of Titan III development
despite a program of stress corrosion control. Tensile stresses (preloads)
on the fasteners are now minimized to 40 percent of yield, and materials are
heat-treated where possible to UTS of 160 ksi. The importance of stress
level, environment, and metallurgical structure of the metal in SCC and HSC
is recognized by the Program Office. Contact with dissimilar metals, the
most likely source of hydrogen from corrosion, is avoided or protected
against. Chemical conversion coatings and anodizing on aluminum, often
retard such corrosion.
NASA plans to initiate studies of service influence on fracture behavior,
i.e., use of fracture mechanics concepts (Ref. 27). NASA has had a few
failures by corrosion in 4330, 4340, AM 355, and 17-7PH.
-2 5-
... ....v -.- .•■ .^ ---. ■ j- :■ . ^i^:,,,^^i^^^aijäaai^^^^^,.i.^^^^h±iiM-iMiWmTi ij^iumiutusuaiM lirti'^limYrWrrfimiVririT'WW^
![Page 37: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/37.jpg)
- , ff^pp^M^^^^
^ ^ n) «, -n « o ^
« UJ h u
■ r-t
^ 0) >
I—I
£
c
H
C c tn
>-. it) c 0)
tn
(U .—i
H
(U o
ß o
Ü
.—I
a
CO
H D -H
tn tn (U 5
u a
tu X u o
Ö
u (0
*-*
U u CO
■ H •—I o tn
a (D
^ ■4-1
0) XI T-,
" 'S r-l 3 O CT
-w C
M ^ ni a) tu JH X o CO u
Ü
bO
a, o u
U
>
O u
a (T) f-i
OJ "+-1
^ h Ü O u 4-3
in X o
0
o oo
U CO X
> t—<
>
o IT)
U U co
c r-H
a< a ü
u U CO .rt
X ö >
bo
o
tn
tu
o
s ffi X OH Oi
i in
1 Ü o
-»-4
in m t-- ^ ■rt ■»H ■»-( ■^ X
u Ü en
tn rti bO
O
u CO
0 Si Xi a c 0 (U at (U 0 4J
0
b tn tn rt) X r Ü
0) ^ tn t3 13 r-H (I) ^ O dj ni nJ U ^ Ü -o^J u cu
Mar
man
co
ole
r
Ü 0 fi JQ O r" Ü
^-1 r-H
O O co x> F
uel
a
ass
eni
td
4->
U
U
(Xi
N
•r-l r-H
O CO
9H
"? IN
i-J l\J
Ü u
> r-H
>
tn tn
rt
Ü
o 4->
o a 0)
ri4 u o SH
xt • rH r-1
O
•rH ,u tn O
m o
■ rH
tn • rH
tn
o o • rH
tn X
u IN]
tM m
u
o oo ■r-H
o oo
O oo
Qi ^
i T-H
r- ro TH •&
-26.
j ..>.>. i. , i M r^-ffirB.TäP'^^^^^^ |g|MMg||j|Miai||gHB|jB|aaB||^^
![Page 38: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/38.jpg)
V. THE PROMISE OF FRACTURE TOUGHNESS CRITERIA
Improvement of analysis of fracture in various environments through
the use of fracture mechanics allows microscopic study of the fracture pro-
cess (whether by SCO or HSC) independent of the influence of specimen geo-
metry effects and dependent only on stress level and environment. The
fracture toughness approach gives, for the first time, a quantitative knowl-
edge of the effects of a particular environment on a steel stressed below the
yield stress. Such quantitative data v/ill be required by the designer once
he learns how to use it. This method reflects the behavior of a metal in an
environment that may lead to either SCC or IISC and does not differentiate
between mechanisms leading to failure.
The KjgQQ parameter, hence, indicates with good reproducibility the
stress-crack-size threshold below which subcritical cracks will not propa-
gate to a critical size leading to catastrophic failure in a gaseous, liquid or
complex environment in a period of usually 500 to 1000 hours. Both KIQ
and KTC,r,~ have units of ksi \ in. Both K's are also independent of specimen
geometry.
Because smooth test specimens require long times for crack nucleation,
Brown (Refs. 28 and 29) and others have used specimens with preexisting
cracks, thus eliminating the crack initiation periori during which surface films
break down and pitting starts. The use of these specimens reduces the likeli-
hood of erroneous conclusions that alloys are immune to SCC (they may not
pit in the test environment, and pitting is generally prerequisite to SCC) and
permits the use of fracture mechanics concepts. Brown introduced the con-
cept of the threshold, KTC,pp. Very quickly Brown's idea became popular,
and many investigations have shown the value of this approach. 4
The use of plane strain fracture toughness criteria, i.e., K.,, and
K „, makes it possible to select fastener materials that are not susceptible
The term plane strain conditions refers to the square fracture produced by SCC or HSC. Plane stress conditions would involve slant or shear fractures, which are not ordinarily observed with SCC or HSC.
■27-
^.;,.,,:—.,.■.:.,■■.,..,■, J^,.^,>^.,Ji»l.J..ttMJ«a^J.^-,;,.„.^.., "Tir'-tnfnaaifiv aaaiaaa ..-■^^.■.— ,.■..■......■ ,. ;■.-.„■„ ..-.■. .,.. ..^..J t^j^si^iUitätSSäStiSIltiäm
![Page 39: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/39.jpg)
- ^-.^lasaw^^ ^iPpgi^?lBTW','^^!L^'l'''J^l?^'w?^I^y!-v*JR^^'Tr;Tg''^''"";T"TriI.y7?
to cither SCC or HSC on the launch pad or in any other environment. The
fracture mechanics approach can show whether a metal is affected by the
stress environment and to what degree. The analysis also shows that where
degradation occurs there is a threshold stress below which no SCC or HSC
occurs, as shown in Figure 5. Note how severely the salt environment
reduces the stress intensity factor K (Ref. 30).
In tough alloys, failure occurs after longer time intervals. Crack propa-
gation may be slower, and the alloy may tolerate a longer crack before frac-
turing. A small crack may cause SCC in a material of low toughness, whereas
a larger crack may be required to fail a tougher material. The tougher mate-
rial may require a longer time to fail because crack growth is slower in a
tougher material and not because SCC or HSC is slower. Time to failure thus
can be used as a measure of SCC growth.
Relating the environmental applied stress intensity factor Krc,pp to the
plane strain fracture toughness K „ permits normalization of the differences
in toughness or heat treatments of alloys . The ratio KTC,rp/K,„ serves as a
normalizing parameter for comparison of steels and their heat treatments.
Figure 6 shows the delayed fracture characteristics of 4340 steel heat-treated
to various strength levels in distilled water (Ref. 31). Figure 7 shows the
same data of Figure 6 normalized by use of the stress intensity ratio
KISCC/K1C-
Stress corrosion tests using precracked specimens have assumed in-
creasing importance in the aerospace industry. These tests are useful to
the designer, the engineer, and the metallurgist. A knowledge of KTr, and
KTC,r„ is important for structural design.
Distilled water and moisture in the atmosphere are seldom considered
to constitute an aggressive environment, yet moisture can have a controlling
influence on the fracture behavior of high-strength steels. The growth of a
crack from an experimentally induced flaw (e.g., EDM-Electro-discharge-
machined slot) was studied by Johnson and Willner (Ref. 32), who found rela-
tionships between the crack growth rate and the crack tip under varying
-28'
^Hj^tiiH^timmiaasästitttBi&BMiBliiiitti&ästtW KH^jggggaBMaBttMiii jggij^giijmimguggmgmi
![Page 40: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/40.jpg)
Wf^s^wg^g-M^^MVuSiiyw'.^^ --■.■ ' .,T- . i ij ji; »^i, j-f^ p »%,. ■ 7', ^•-."■T-kr'fS'w^wB^v*- -w ** ra »TI- ■■ ■. i f'T.' ■.'-'
120
[^100
" 80
4340 STEEL HEAT TREATED TO 225 ksi UTS
PRECRACKED SPECIMEN EXPOSED TO 3 1/2% NaCl SOLUTION
UNTILEVER BEAM LOADING
T FAILURE CAUSED BY SUBCRITICAL CRACK EXTENSION BY STRESS ENVIRONMENTAL' CRACKING THRESHOLD
Li NO FAILURE
I02 t I03 I04
TIME TO FAILURE, mm
Figure 5. Typical Behavior of a High-Strength Steel in a Corrosive Environment (Ref. 3)
I0;
■29-
■■...".■■--■ ■■ .,n,;i—,<i.ii„v----t-i.;.^.;•,■■,■■•:,.,, ,, ■ ..:.-:..-..,../;.-.^)^-a.j^.j^^w-a.^^;. ■.^■■^^..^.i^.^ju.:..-,..,. ;,,.a- ^„.^..^„.^..A ^-..^..^^.y^^^v,,:.,, jagj ■ —^^-■ ■'-"■-*1"li|iftMiMi
![Page 41: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/41.jpg)
mmfr?*' r^mi. i wnj&^M&i -rrt.rfi*-jt***mif)VqHfH,7~.lv'*'T'--
160 r
140
120
^ 100
>-'
^ 80 UJ
CO
UJ en
60
an 40
20
0 U,
4340 STEEL HEAT TREATED TO INDICATED LEVELS
PRECRACKED SPECIMEN EXPOSURE DISTILLED WATER
CANTILEVER BEAM LOADING
'0
■265ksi UTS
232 ksi UTS
10 10' 10- 10'
TIME TO FAILURE, mm
Figure 6. Delayed Fracture Characteristics of 4340 Steel at Var;jus Strength Levels Resulting from Exposure to
Distilled Water (Ref, 31)
-30-
■ - ■ ' -— - ' ' ■'^'■■:-- ;- n'lij-imitilitl^iitiiitWliilittfliiillltlllllitlinim'aiiilli i i i -■•Tiifinr-i -■--■ -••■^■-.-, - .—:■
![Page 42: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/42.jpg)
mmmmmmmm.
265 ksi UTS
10 I02 I03
TIME TO FAILURE, mm
10'
Figure 7. Data of Figure. 6 Normalized by Use of the Stress Intensity Ratio (Ref. 31)
-31
«aj^^au.^^to^^^ ] i^ iiii'MMiaiiggiäjiigii —ütüiü m nümmmi -^-.■I..-..-^- .a.w,^^,.^.m(tiril( ^
![Page 43: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/43.jpg)
^|flipi|fl^WWWi*ll^Wlj|l||^IJ>MIMW^ ^wmi^ismmmwvi^mffm^'r<'"-'~ ■'■ ■; ^■v«pwl^B^l^w^lWl^w'.^||^l■^fl^l^f^y^|l|\^y^^a^H8SSt!fii",?'^°'^
conditions oi'liquid water, water vapor, and temperature. The work was
conducted with an 11-11 steel heat-treated to a strength of 230 ksi. Water
vapor had a marked effect on crack growth at constant load; crack growth
changed as humidity was varied. The crack propagation in water or water
vapor is consistent with crack propagation mechanisms of either SCC or HSC .
It is highly probable that either mechanism can occur in high-strength steels
and that the chemistry of the aqueous environment determines which mech-
anism is operative. In this instance, however, it is very likely that corro-
sion occurs on this steel and hydrogen enters the metal (Ref. 33). Hanna,
Troiano, and Steigerwald (Ref. 7) have also presented evidence that HSC
occurs with distilled water; the hydrogen is supplied by the cathodic reaction
of a corrosion cell. In addition, the crack growth rate activation energy of
9000 cal/mole agrees fairly well with the known value for the diffusion of
hydrogen in iron (Q - 7800) (Rcf. 34), which also supports the findings of
Johnson and Wilner.
Since both SCC and HSC can occur in aqueous environments, it is sur-
prising that the operative mechanism appears to depend on the nature of the
steel. Benjamin and Steigerwald (Ref. 35), using fracture toughness analysis,
exposed two high-strength steels to distilled water and 1 . 5I\' and 3. ON NaCi
aqueous solutions. Distilled water was found to be a more agressive environ-
ment than the salt solutions for 4340, and the reverse was true for HP-9-4.
Using supplementary polarization experiments, they found that delayed failure
in 4340 was the result of HSC. The behavior of the HP-9-4 steel, however,
was consistent witli the SCC mechanism, with anodic dissolution occurring
along active paths.
The type of data obtained by fracture mechanics analysis is illustrated
by the work of Freedman (Ref. 36), who obtained K.,, and K „ data on
ferrous and nickel alloys. Single-edge notched and fatigue-cracked specimens
were tension-loaded in a salt solution for 1000 hr (accelerated test). Identical
specimens were tension-loaded in racks exposed at the seacoast (Playa del Rey,
California). Times to failure at seacoast varied from 49 to 7668 hr. Some
specimens were tested for 12, 843 hr without failure.
•32
i ■ -■- ■-■.- :--■- ■....-. ■-■~l: aaaMaBüaaiüi i ^-■-.^^^^^^i^xv.m,,,,.^-^^.»,«^:«,:. ■ -■> ..^^.^^.v,.,..^-^,^^^^^^^^^^^^^^^....^.
![Page 44: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/44.jpg)
»p :,«K^--r»"T«*,",i ■■■nMiPBpgiBS^^iaBswPBwgg^^^ .«r-r -"---rri^lLjJIUJ^I
Freedman's data (Table 7) ^ive a rating of the susceptibility of various
alloys to accelerated (laboratory) and sraroast testing; the ratio KTC,rr/K r
for seawater ranks the alloys from Inconel 71K (most resistant) to sensitized
Type 304 (most susceptible). There are unexplained differences in the ratio
for the accelerated test, which can probably be attributed to the variability
of the aggressive environments.
Additional data on the stress-corrosion properties of the precracked
high-strength precipitation-hardening stainless steels were obtained by
Carter (Ref. 25). These data (see Table 8) showed that the precipitation-
hardening stainless steels (e.g., 17-7 FH and IJH 15-7 Mo) were particularly
sensitive to SCC. Most martensitic steels were very resistant, with
^ISrr^IC Vt""v r'OSl' io unity. Steels with low K' „„ values had low K ,r •
All failures were intergranular.
Overaging was found to increase fracture toughness and stress-corrosion
resistance. As might be expected, comparison of data for precracked speci-
mens and smooth specimens revealed discrepancies.
Comparison of Freedman's data with iho.se of Carter and ro-worker."-
is not possible because of the different alloys tested. In only two cases arc
the data comparable: AM355 SC J" 1000 and 17-4 lJil H900. There exist wide
and unexplained differences in the K.i.rr/K ratios.
The effect of high-pressure (5000 psi) hydrogen on Inconel 7 18, Inconel
625, A286, AISI 347, Ti-6A1-4V and Ti-5Al-2.5Sn has been studied by fracture
mechanics analysis (Refs. 37 and 38;. Of the group, Inconel 718 and A286
were niost resistant, while Inconel 62 5 was most embrittled.
-33.
W.iVl&i ri^id'tim; i*: LH i* [anfljaBaanaaaaiiBBaai :£u. anJ^mMM«i■TrMtl^^^''^:"';J"^l■^^°''Jii,
![Page 45: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/45.jpg)
'Yrf^t^^'r^f^^^t J IJt II«!)»
Table 7. Fracture Toughness Rating of Alloys and Heat Treatments lor Resistance to Saltwater Environments (Northrop Data, Ref. 36)
Seaco^s 1 OBt Accel erated Test
Material Heat Treatment UTS. ksi 'Sscc ^ SCC/K]C K1SCC KISCC/K1C
Inconel 1950,F AC, 8 hr 189 t 106 0. 87 130 0. 98 718a 1350' + FC to
1200'F for 24 hr
17-4 PHa H 1150 151. 6 93. 9 0. 77 I 10 0. 89
AISI 304 Annealed 84 0 53. 5 0. 77 59. 7 0. 86
4340 800^ .'empered 204 8 48. 3 0. 72 29. 7 0. 44
17-4 PH H 9C0 202 4 38. 5 0.69 40. 3 0. 72
H-l 1 (AM)b 1 lOO'F Tempered 232 6 39. 5 0.62 23 2 0. 24
410a 1 125*F Tempered 128 a 52. 4 0. 55 49, 6 0. 52
H-l 1 /AM)b 1000'F Tempered 300. 3 16. 7 0. 52 H. 6 0. 27
18 Ni USO) 900 "F 269 5 55. 6 Ü.50 72. 9 0.65
H-ll (VM)b 1000'F Tempered 114 0.40 10. 8 0. 38
4340 475^ Tempered 267 2 1 3 3 0 29 11.1 0. 24
AM 35S (FH)b SCT 1000 33. 1 0. 28 50. 3 0.42
AM 355 SCT 1000 169 4 24 5 0. 24 36. 7 0.43
410 650'F 7 empered 197 Ü 22. 0 0. 24 25. 8 0. 26
AM 355 SCT 850 195 9 10. 7 0.22 24. 9 0. 52
AM 355 (FH)b SCT 850 9.7 0. 15 6 2 0. 10
AISI 304 Sensitized 100 hr 1100'F
83 9 8. 5 0. 12 15. 2 0. 22
Plane strain conditions maintained only at low stress intensities. Therefore, values are approximate. True plane strain K.-^,- could not be obtained.
AM = air melt, VM = vacuum melt, FH = fully hardened.
34-
a^...,---.......^ ■ a imaMiMii—Mü—I ^-"—'-■"—■ - ttttammttm
![Page 46: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/46.jpg)
—pry^tijBW.Ha^yiBMEBMeivJ«^^^ ^v^,'^'''••'•''""•' "^v»---"'"-""■"■•■■'■—'"-•'■■•''
Table 8. Fracture Toughness Rating of Alloys and Heat Treatments for Resistance to Saltwater Environments (Boeing Data, Ref. 2S)
Material Heat Treatment UTS, ksi Kiscc/Kr
AM 35.i SCT 1000 178.0 1.00
AM 351- SCT 1000 Modified 173.4 1.00
AM 364 H 950 191.5 1.00
17-4 PH li "no 194.6 1.00
17-4 PH H 1000 162.2 1.00
15-5 PH {AM)a H 1000 161.6 1.00
15.5 PH (VM)a H 1000 162.9 1.00
PH 13-8 Mo H 950 225. 1 1.00
Custom 455 H 950 247.0 1.00
15-5 PH (AM)a H 900 195,7 0.83
AM 362 11 1000 178.'» 0.77
15.5 I'll (VM)a 11 9ÜÜ rn.5 0.7 5
AM 364 11 850 188.7 0.71
17.7 PH RH 950 186.5 0.59
PH 15-7 Mo TH 1050 178.2 0.55
AM 355 SCT 850 213.5 0.55
PH 15-7 Mo RH 950 219.4 0.44
AM 362 H 900 200.5 0.41
17.7 PH TH 1050 197.2 0.41
AM - air melt, VM = vacuum melt.
![Page 47: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/47.jpg)
"f-^£*J? jHiB.41^J4H|iL-l»t||^l^ljlMWWIlJPW^
UI'HIIIIK öl SUHI .11 tii-d - Load Kxpc r I mmt S with Notclicrl Specimens of Various Uli rn-Hijjh-St rcngtli Steels Exposed to a 5% Salt-
'o(4 Atmosphere (Kef, SI)
UTS Appln-.l Numlie r of fa i hi res
it.-el Rant;c St rcsfi, 1 yp«* ..1 Coat ipy in 1000 hr/N. imiie r ksi kBia of Spec imens T< sted
4 (4 0h ^f,0-2H0 16 1 Not plated 1/1 A i-lO1' 26O-2H0 16 1 l.i.w H Cd pUtcd 1/3
1 MO"-' 2 60-?. K0 161 Not plated 1/3
■1 140 Zt,0.2H0 163 l.i.v.- II Cd platrd i/i 4 140 1 HO-200 120 N'.l plated 0/1 4 14 0 1HO-200 120 \'.ii iiutn- deposit cd Cd 0/1
4 UOM J20-240 142 Not plated 1/3
4 1 !0M 220-240 142 Low II Cd plated 2/1
11-11 2HO. iOO 17', Not plated 1/i II. 1 1 2K0- uin 17'- I.nw II C.tl plali'd 2/1
II 1 1 .'HO- 100 1 ;'• N 1 Id pl.ll e.| 2/1 II II .'i.O .'HO 11. Not plated 1/3
II 1 1 2 Ml- .'HO 16 i I.ow !l 1 d plated 6/1
II 1 1 .'(.0 .'Ml) 16 < N i ( d [ilat ed 0/3
l)i..i> 2H0- 100 171 Not plated 1/1 l)6ai 2H0- 100 1 71 \' at until - depo.s it ed id 3/3
Pba. 2(.0-2KO H.1 Not plated i/3
Dfcac 2(>0-2H0 It. 1 V aru im - deoos itcd Cd 2/3
D6ar 220-240 142 Not plat ed 3/3
n6ac 2 2 0-240 142 Vacuum-deposited Cd 3/1 D hat- 220-240 142 Ni-Cd plated 0/3
HP-r»-4- 4^ 260-2H0 M'1 163 Not plated 3/3
IIP-rf-4- 4^ 260-2H0 M'l 163 Vacuum-deposited Cd 1/3
IIP-9-4 4S 260-280 nr 163 Not plated 3/3
HP-'t-4. 4S 260-2K0 n1' 163 Vacuum-deposited Cd 3/3
C-45S 220-240 142 Not plated 0/3
C-4SS 220-240 142 Vacuum-deposited Cd 3/3
r-4ss 220-240 142 Ki-Cd plated 0/3
AFC-77 240-260 142 Not plated 2/3 A FC-77 240-260 142 Vamum-deposit ed Cd 3/3
IHNi (2H0) 2H0- )00 171 Not plated 3/3
ma ra^in B 2K0- 100 171 Vacuum-deposited Cd 3/3
2H0. 100 171 Ni-Cd plated 1/3 IHN,(2S0) 2SO-270 163 Not plated 0/3
ma ranin B 2S0-270 210-270
16 1
It. 1 Vacuum-deposited Cd Ni-Cd plated
0/3 0/3
d
The applied stress was equivalent to about 71"', of the design yield strengths of the steels, except for the marajjinK steels.
Air melted.
"Vacuum melted.
Martensitic heat treatment.
Rainitic heat treatment.
•36-
f^jJifyrtttii^i^t^jM^
![Page 48: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/48.jpg)
^^^^^^r^^mmmmiwum^ +, .!■ m.K,'''.mm>^v^m^m*j^l^wH^w*miw
VI. KKrOMMKN'DATIÜNS
Two major problems related u^ SCC and HSC confront the aerospace
industry: (1) prevention of SCC and HSC and (2) test standardization, data
accumulation, and dissemination of information.
A. PREVENTION OF SCC AND HSC
There are some obvious practical approaches lo the problem of failed
fasteners by SCC and HSC. The first is the use of alternative materials.
There are materialt with good resistance to SCC. On the basis of the frac-
ture toughness criteria, KTC.r„, and the ratio K ...p,,/KT(-, tempered with
experience, a selection could be made. Unfortunately, fracture toughness
criteria are only now being collected and not all fastener materials have been
tested. However, there are some highly co rrosion-resistant materials of
the stainless steel type available, e.g. , A2Hb, A2Hb C\V, Inconel 718, and
Inconei 7 18 CW.
The second obvious solution is to keep the agressive environment or
the hydrogen source away from the steel. Although aerospace engineers shy
away from coatings, platings of cadmium or aluminum may be helpful on
low-alloy steel martensites. Extreme care in electroplating and required
subsequent baking must be exercised at high strength levels to prevent HSC.
In some aerospace applications, organic coatings, paints, Lock-tite, Lock-
safe, greases, or even baked-on solid lubricants can protect against the
environments. Torquing and retorquing on the bolts can remove these' types
of coatings, and reappl icat ion ol the protection is then required.
The resistance to environmental cracking ( S"'. salt log) ol ten high-
strength steels, with and without cadmium or cadmium-nickel coatings,
was studied by Lauchner (Ref. 39); the results are given in Table u. Some
steels, AISl 4340 (180-200 ksi UTS), Custom-455 (220-240 ksi UTS), and
18 Ni (250 ksi UTS), had good resistance to SCC in this environment without
-37.
![Page 49: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/49.jpg)
■P'L-, . HliJfJijlllJJJi^-XI.JAMiJI.IINI Miili IJ nj .....J.^iJIJi J.JMJ11.11. ' H ' n'-. ^UJi-'mjlll .|!1. J... J'.' .. .... '. I.MU.I iil.H.. .I'1.1 _ . ..J ' . J.11 HJHI. .1 . .UM,J.I-1 'Ml. . i . | n.7r--a'J^JP^jr.
i'oatings. Note the superiority of the cadmium-nickel coating to the other
types of cadmium coatings (low hydrogen plated and vacuum deposited).
A less obvious solution to the problem is the use of designs that elimi-
nate or minimize factors promoting SCC and HSC. One should, for instance,
avoid crevices, deep recesses, sharp corners, notches of ai.y kind, and
dissimilar metals unless one metal is insulated from the other.
In any design in which new alloys are to be tried and new environments
experienced, it is highly recommended that fracture toughness tests be con-
ducted to ascertain the possibility of some susceptibility to degradation, if
not complete failure.
L3 DATA COLLECTION AND TEST STANDARDIZATION
There is a need for standardization of fracture toughness tests using
the precrackod specimens. The ASTM already has a tentative specification
on testing (Ref. 3). Without standardization, the available dati have limited
usefulness in material selection or design. A standard test must be in exis-
tence long enough that sufficient data can be accumulated for statistical study.
The accumulated data should be compiled into usable form by industry,
the metallurgical profession, a government agency, or a technical society.
-38-
...^■.^.^.^^-.^^im^ - am i — —-;.-—
![Page 50: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/50.jpg)
'Jf ^i»sT»fs. V* -^J *«J!^
vii. f:()K(:LrsK;::.s
The rurrfiit I ci luiolciu y ul lii uh - st ri'ni'lh Uiblcm-r.s in .(
ajjplications has lircn appraisefl.
While (lu'rc is ,i (hstinct rlil h-rciu i
on the laboratory scale, it is diftn ul
bet v-'ei-n the I \<,
er spat
I), tv/eeii SCC anrl 11S( ■ i>li
It , l f" not tllUOS.Ml,] '•. 1" 'iilNrnii at e " "lee In 111 Mils i n I )ic ! i ( 1,,'. ( III CDS [l HI
■^ • l!'.'| n.IHlien
■i - I1 ' II i I I , 1
• • ( n i n ; i ;,
eiil Iy aflvain ed tu p ri ii i( i tlarit'er.■■!; • I i
nat ions I hal c >.IIM Ie.id If i,111 u r.■.
file Ii i::!i - si '•. IM I Ii la sli-in i--. lh.il
f I I V I (lef 1 i ill ii t ll r i e I Vpi s ul i ,! I .■'."
i ,i I type, .i ml ( . 1 l)\ r i I
, I I I I M 1 Spll ( fl - s .
Kxa tuples ■ 11 I,I 11 ii r es un the 1 .tan III i ■ . i i ■,• •' '. >
na I ii re i I the p ml) lei i .
I'rait ii ri' tuuiihness analysis filers 'he lu ■ I I; 'pi
SCC or IISC. Tile analysis dm s mt " lien nt^.te ',.■!. ■
use of plan«' - st ra in I rai t ure tnut'lmess 1,. . .i IT' ■ ' I ■ .•- I
' h
K . e , ( r i I e r i a M 11 e r s [ i r o m i s < ■ 11 s e 1 e i i ,; ; i ;, •:, i ■ ■
SMS« ept lb le to «SCC .ir I ISC |,| i hires. I i . I , , . I ■ . ., '1.(1
hei om inu ' i M i r-1 ■ i in a lli n i.' I ii 1 to I hi' '1
1 '■ i ^ not .-,. j f f
' * r i ■ , 11,! i
i : ,ii ■ i i' ■ ,; n ■ ■ i
I r-'e Ml..-, , ,,| ,1,1:1.,, ,,, ,
•M, I, . I| ■'■ • i M tile
■ ' ! ' !'■ i ho , ,,l , •1 fea , bei oi: i I h,- ,. ii i ■.i s 11 r, ■- I lily lurina n<
!l I'L' 'i.it.i ,,n
:.-::■ s f J,
liil-l ' MJli
■;. ' . •■,• ,,.,1
■■'■. oi !,,.;, ,r
i si ion |,n
«^■-^-^-■■ -*. ■-■- —- ..-..--^■— ■■ --■*- -■ -■■ —"TirtnMiiH^tniii.i , ■■■- -— --.-■-. ..■--..~J.
![Page 51: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/51.jpg)
ssssr«!^^;""'-^"? r^^i^'r-Tic-•>!> T^<^ii¥|nqrFl^«JiH.l'!W..'J'^^'^^
REFERENCICS
1. A.C. Hood, "Preventing Stress-Corrosion Cracking in Threacled Fasteners, " Metal Prog. Q_l_, HS-«8(1067).
2. J. K. Stanley, "Solutions to Some Stress Corrosion Cracking Problems in Aerospace Situations," Proc. Joint Aerospace Marine Corrosion Tech. Seminar, First, NACF, Houston, Texas ( j %9).
3. B. F. Brown, Stress Corrosion Cracking: A Perspective Review ul the Problem, NRL7I30, U.S. Naval Research Lab., Washington, DTT. (16 June 1070).
5.
F.K. Fletcher, W.F. Berry, and A. R. Klse.i, Si ress - To r ros iun Cracking and Hyd rogen-Sl ress Parking of High SI rcnglh Steel, I) MIC ZiZ, Battelle Memorial Insl. , Defi-nse Mi.'tal Iniurmation Center, Columbus, Ohio {29 July 1''()()).
H. L. Logan, The Stress Corrosion of Metals, John Wiley and St-ns, Inc. , New York ( 1066).
6. A. R. Elsea and E. E. Fletcher, Hydrogen Induced Delayed Brittle Failures of High Strength Steels, DMIC [9b, Battelle Memorial Inst. , Defense Metals Information Center, Columbus, Ohio (20 January 1(:'64).
7. G. L. Hanna, A.R. Troiano, and E.A. Steigerwald, "A Mechanism for Embrittlement of High Strength Steels by Aqueous Er.vi ronments," Trans. ASM 57, 658-671(1064).
H. K. Ma/.anec, and R. Seinoha, "Delayer] Fracture in Ma rt ens ite, " Trans. AIMEZV-), 1 602-1 (.OK ( 1 965).
10.
B. F. Brown, Si ress-Co r ros inn Cracking and Related Phenomena in High Strength Steels, NRL 6041, U. S Naval Research Lab. , Washington, D. C. ( 1063).
H. J. Bhatt, and E.H. Phelps, "Effect of Solution pH on the Mechanism of Stress Corrosion Cracking of a Martensitic Stainless Steel." Corro- sion 17, 430-434 (1061).
11. N. A Nielsen, "Observat ions and Thoughts un Stress Corrosion Mechanisms," Corrosion 27, 173-HO (1971).
Preceding page blank -41
a.t^a^^.^yiaabMaM^a^^ . ..-,...■... „„,BJ-^^^.....a- ^^-^■'- ^
![Page 52: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/52.jpg)
lilKilPIPIIP SflflJFBj L-Wl^SiT^TTliT
12. I. Matsushiina, A. Dee^an, and H.II- Uhlig, "Stress Corrosion and Ilydroiicn Cracking of 17-7 Stainless Steel," Corrosion 22, 23-27 ( l'r'66).
13. D. L. Dull and L. Raymond, "A Method of Evaluating Relative Sus- ceptibility of Bolting Materials tu Stress Corrosion Cracking," Paper presented Westcc Conference (March 1^72).
14. A. Phillips, V. Kerlin.s, and R.V. Whiteson, Electron F ractographic Handbook, ML-TDR-64-4 1 6, Air Force Materials Lab. , Wright- Patterson Air Force Base, Ohio ( 1964).
15. J. P. Fidelle, J. Legan, and C. Couderc, "A Fractographic Study of Hydrogen Gas Embrittlement in Steels," Trans. AIME (1972)(in press).
16. N. A. Tiner and C. B. Gilpin, "Microprocesses in Stress Corrosion of Martensitic Steels," Corrosion 22, 271-279 (1966).
17. H. Suss, "Stress Corrosion - Causes and Cures," Mater. Design Eng. 6j_, 102-148 (1965).
18. J. Bourrat and J. Hochmann, New Austenitic Stainless Steels Resistant to Stress Corrosion in Chloride Media, Aciers Speciaux, Monographies Techniques, No. 9(1964).
19. F. R. Bloom, "Stress Corrosion Cracking of Hardenable Stainless Steels " Corrosion 11, 351-361(1955).
20. .I.E. Truman, R. Perry, and G. N. Chapman, "Stress Corrosion of Martensitic Stainless Steels," J. Iron Steel Inst. (London) 2 02, 745-756 (1964).
21. E.A Drey er. Investigation of Susceptibility of High Strength Marten- sitic Steels to Stress Corrosion, ASD-TDR-62-876, Aeronautical Sys- tems Div. , Wright-Patterson Air Force Base, Ohio (19b2).
22. R.T. Ault, R. B. Holtman, and J. R. Meyers, Heat Treatment of a Martensitic Stainless Steel for Optimum Combination of Strength, Toughness and Stress Corrosion Resistance, AFML-TR-68-7, Air Force Materials Lab. , Wright-Patterson Air Force Base, Ohio (1968).
23. P. Lillys and A. Nehrenberg, "Effect of Tempering Temperature on Stress Corrosion Cracking and Hydrogen Embrittlement and Marten- sitic Stainless Steels." Trans. ASM 48, 327(1956).
-42-
fbätBtmamätmamaäiitSt mmmmsäsmamuaaaattiMtaUMSitKliM jMaMMiflHHmMyaiMBMgEi
![Page 53: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/53.jpg)
PIPBWWWP!»!! wmm^wtmimm
E. H. Phelps and A. W. Loginow, "Slrcss-Corrosion of Steels for Aircraft and Missiles," Corrosion 16, 325-3351(1969).
25. C. S. Carter, D. G. Farwick, A.M. Ross, andJ.M. Uchida, "Stress Corrosion Properties of High Strength Precipitation Hardening Stain- less Steels," Corrosion Z7, 190-197(1971).
26. Design Guidelines for Controlling Stress Corrosion Cracking, NASA 10M33107, Marshall Space Flight Center, Huntsville, Alabama (1970).
27. W. R. Lucas, Chairman, Report of the NASA Ad Hoc Committee on Failure of High Strength Materials, Marshall Space Flight Center, Huntsville, Alabama ( 1971).
28. B. F. Brown, "A New Stress Corrosion Cracking Test for High Strength Alloys, " Mater. Res. Std. 1_6, 129-133(1966).
29. B. F. Brown, Stress Corrosion Cracking and Corrosion Fatigue of High Strength Steels, DMIC 210, Battelle Memorial Inst. , Defense Metals Information Center, Columbus, Ohio (1964).
30. B. F. Brown, "The Application of Fracture Mechanics to Stress- Corrosion Cracking," Mefjyjl_urj^£aJ_J^ 13, 17 1-18 3(1968).
31. J.H. Mulherin, "Stress Corrosion Susceptibility of High Strength Steel in Relation to Fracture Toughness," Trans. A5ME, J. Basic Eng. 88, 772-782(1966). —-._-.-——_— - —.
32. H. H. Johnson and A. M. Willner, "Moisture and Stable Crack Growth in a High Strength Steel," Appl. Mater. Res. 4, 34-40(1965).
33. N. J. Norton, "Diffusion of D2 from D2O Through Steel," J. Appl. Phys. 24, 499 (1953).
34. E. W. Johnson and M. H. Hill, "The Diffufivity of Hydrogen in Alpha Iron," Trans. AIME 218, 1104-1112(1960).
35. W. D. Benjamin and E. A. Steigerwald, Stress Corrosion Cracking Mechanisms in Martensitic High Strength Steels, AFML-TR-67-98, Air Force Materials Lab. , Wright-Patterson Air Force Base, Ohio (1967).
36. A. H. Freedman, Development of an Accelerated Stress-Corrosion Test for Ferrous and Nickel Alloys, NOR 68-58, Northrop Corp. , Norair Div. , Hawthorne, California (1968).
-43-
f,:Jt»JMaL^i,^,.^»rf.».,-:^,.«J,,a„-.^^ mj|gjagBaaaBjiMg|gM^||gjgggjg|jg||gg|g|i|y
![Page 54: Stress Corrosion Cracking and Hydrogen Embrittlement of ... · fasteners in aerospace equipment as a result of SCC or HSC occurs infrequently and almost always unexpectedly. There](https://reader031.vdocument.in/reader031/viewer/2022040211/5e6cf5ec3b759119e64270a2/html5/thumbnails/54.jpg)
SSa«?S«!BP5SäiHB?Hp JIJIIWJJWiMlWMIgiHBfW^^
37.
38.
39.
J. A. Harris Jr. anrl M. C. Van Wanderhan, Properties of Materials in High Pressure Hydrogen at Cryogenic, Room and Elevated Temper- atures, PWA FR-4566, NAS 8-26191. Pratt and Whitney Div Aircraft Corp. , West Palm Beach, Florida (1971).
United
R. J. Walter, H. G. Hayes, and W. T. Chandler, Influence of Gaseous Hydrogen on Metals, R-8719, NAS 8-25579, Rocketdyne Div. , North American Rockwell Corp. , Canoga Park, California ( 1971).
E. A. Lauchncr, The Stress Corrosion Resistance of High Strength Steels for Bolting Applications, NOR 69-91, Northrop Corp., Norair Div., Hawthorne, California (1969).
n