![Page 1: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/1.jpg)
ARGONNE NATIONAL LABORATORY ANL-92/289700 South Cass Avenue, .Argonne, lUinois 60439
Distribution
Categories:Materials (UC-504) and
ANL--92/28 Nuclear Waste Management
I_92 019239 (UC-51 0)
STRESS CORROSION CRACKING OF CANDIDATEWASTE CONTAINER MATERIALS- FINAL REPORT
j. Y. Park, P. S. Maiya, W. K. t_oppet, D. R. Diercks,W. J. Shack, and T. F. I_'Issner
Materials and Components T,_chnology Division
June 1992
Work sponsored by
U.S. DEP__NT OF ENERGY
under subcontract from Lawr_nce Livermore National Laboratory(ACK 85861)
![Page 2: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/2.jpg)
Contents
AIx_L ..........................................................................................................................................................1
1 Introductton.........................................................................................................................................2
I. 1 Objectives............................................................................................................................... 2
1.2 _und ............................................................................................................................ 2
2 Test Materials ...................................................................................................................................... 2
3 Sl_Rate Tens_ Tests ................................................................................................... 3
3. i _ental Prcx.'edur_ ................................................................................................ 3
3.2 _ Results fl'L_ksW- I {W-22) .................................................................................. 12
3.2. I Observations d SCC by SEM ............................................................................ 12
3.2.2 Esttmatlon of L_al Plmstlc Strains ................................................................ 16
3.2.3 Relative SCC Susceptibility of Waste ContainerMa_ .................................................................................................................. 24
3.2.4 SCC Susceptibility of Weldment Specimens .............................................. 26
' 3.2.5 Influence at"Strain Rate on SCC..................................................................... 3 I
3.2.6 Measux_ment of Crack Depth in SSRT Spectmerks ................................ 3 l
3,2.7 Influence of Water Chemistry on SCC.......................................................... 31
3.3 S,._tT Results (Test.sW-2_/W-3,3) ............................................................................... 32
3.3. I Crack Depth Distribution in SSRT Specimens .......................................... 32
3.3.2 Relative SCC Susceptibility o[Waste ContainerMaterials .................................................................................................................... 39
3.3.3 Influence of Strain Rate on _ ...................................................................... 51
3.4 Preparation and Aria.]yses of Test Solutions ............................................................... 51
3.5 Measurement of Elec_emlcal Potential ............................................................. 57
4 Fracture-Mechanlcs Crack-Growth-Rate Tests ...................................................................... 61
4. I _ental _ur_ ................................................................................................ 61
4.2 _ and _t_ons .................................................................................................... 64
4.2. I _d--Ratio Tests .......................................................................................64
4.2.2 Lo_-Load-_Tests ........................................................................................ 65
5 S_ranmy ar_ Cauclus_ns .............................................................................................................. 66
6 ,_flcn_ents .............................................................................................................................. 73
7 Ht_'_ ............................................................................................................................................. 73
i
|i_ iii
_n
![Page 3: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/3.jpg)
Figures ............................ _..........__ _ _ ,........1 Fabrication Drawing for Base Metal SSRT Specimen ....................................................... 10
2 Fabrication Drawing for Gas-Metal-Arc Welded Specimen ........................................... I 0
3 Fabrication Drawing ibr Electron-Beam-Welded Specimen ......................................... 1 1
4 Schematic of SSRT Setup with Feedwater and ElectrochemicalPDtentlal Monitoring Systems .................................................................................................... 1 1
5 Cross--Sectlonal View of Drilled Hole in SSRT SpecLmen ............................................. 12
6 SEM Photomicrographs of Hole Regions of Type 304L SS and Incoloy. 825 .......... 15
7 SEM Photomicrographs of Hole Regions of Welded Incoloy 825Inked alter _p= 2,3% ........................................................................................................ 18
8 SEM Photomicrographs of Cracks in Hole Regions of Cu andCu-Base Alloys................................................................................................................................... 19
9 SEM Photomicrographs of Cracks in Hole Regions of Welded Type316L SS Inten'upted a_er £p 3.0% .......................................................................................... 19
10 SEM Photomicrographs of Cracks in Hole Regions of Welded Type316L SS [ntemJpted after _p = 3.0% ....................................................................................... 20
] I SEM Photomicrographs oi"Hole Regions of Incoloy 825In_ after _p= 3.0%.......................................................................................................... 2 0
12 SEM Photomicrogx'aphs of Hole Regions for Incoloy 825 and Cu-30% Ni.............. 2 1
13 Strain Concentration Factor as a Yunctlon of Plastic Strain for Cu ............................. 2 3
! 4 Strain Concentration as a Function of Plastlc Strain for Type 316L _ .................... 2 3
15 Relative Cracking Susceptibility of Stx Candidate Materials In SimulatedWeUJ-- 13 Water at 93°C............................................................................................................... 2 6
16 Relative Cracking Susceptibility of Stx Candidate Materials in SimulatedWell J--13 Water at 93°(3................................................................................................................ 27
17 Comparison of SCC Susceptibility of Type 304L SS Base Metal andWeldment Specimens in Simulated J-13 Water at 93°C ................................................ 27
18 Compark=_on of SCC Susceptibility of ,Type 316L SS Base Metal andWeldment Specimens in Simulated J- 13 Water at 93°C ................................................ 2 8
19 Comparison of _°-43CSusceptibility of Incoloy 825 Base Metal andWeldment Specimens in Simulated J-13 Water at 93°C ................................................ 28
2 0 Comparison of SCC Susceptibility of Cu Base Metal and WeldmentSpecimens in Simulated J- 13 Water at 93°C ...................................................................... 2 9
2 1 Comparison of SCC Suscept ibflity of Cu-30Ni Base Metal and WeldmentSpecimens in Simulated J-13 Water at 93°C ....................................................................... 29
22 Comparison oi' SCC Susceptibility of Incoloy 825 Incoloy WeldmentSpecimens with Two Different Filler Materials In Simulated J-13 Waterat98_ .................................................................................................................................................. 30
il ,v
![Page 4: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/4.jpg)
23 Comparison of SCC Susceptibility of Cu-7AI Base, Electron.-Beam--Welded,and Gas-Metal-Arc Welded Specimens in Simulated J-13 Water at 93°C .............. 30
24 Effect of Strain Rate and Specimen ECP on SCC Susceptibility of Type304L SS in Simulated J-13 Water at 93°C ............................................................................ 33
2 5 Effect of Strain Rate and Specimen ECP o11 SCC Susceptibility of Type316L SS in Sin_ulated J--13 Water at 93°C ............................................................................ 33
26 Effect of Strain Rate and Specimen ECP on SCC Susceptibility of Incoloy825 in Simulated J--13 Water at 93°C ..................................................................................... 34
2 7 Effect of Strain Rate and Specimen ECP on SCC Su_eptibflity of Cu inSimulated J- 13 Water at 93°...................................................................................................... 3 4
28 Effect of Strain Rate and Specimen ECP on SCC Susceptibility of Cu-7Alin Simulated J--13 Water at 93_C.............................................................................................. 3 5
29 Effect of Strain Rate and Specimen ECP on SCC Susceptibility of Cu-30Niin S_nulated J- 13 Water at 93°C .............................................................................................. 3 5
30 SCC Susceptibility of Incoloy 825, as Indicated by Stress Ratio for Testswith DifFerent Water Chemistries under Approximately the Same ECP_nsat 93_C........................................................................................................................... 36
3 1 SCC Susceptibility of Cu in Terms of Stress Ratio for Tests Conducted inSimulated Water without and with _1.0 ppm H202 at 93°C ............................................ 3 6
32 Crack Depth Distribution on a M.,etallographically Polished Surface of a"IY-ans_.rsely Sectioned Type 316L SS Specimen ............................................................. 3 8
33 Maximum Crack Depth as a F_nctlon of Material Removed for SSRTSpecimens .......................................................................................................................................... 38
34 Nominal Stress versus Plastic Strain for Incoloy 825 Specimen inSimulated J-13 Water at 93°C .................................................................................................... 4 1
35 Nominal Stress versus Plastic Strain for Cu-30Ni in Simulated J-13Water at &cY_C.................................................................................................................................... 4 1
36 Variation of Stress Ratio with Plastic Strain Ibr Incoloy 825 in SimulatedJ-.13 Water at 93°C .......................................................................................................................... 42
37 Variation of Stress Rallio with Plastic Strain for Cu-30Ni in SimulatedJ-- 13Water at 93_ ......................................................................................................................... 4 2
38 Nominal Stress versus Plastic Strain for Type 3¢)4[, SS in Simulated-F-13Water at 93°C .......................................................................................................................... 4 3
39 Variation of Stress Ratio versus Plastic Strain [br Type 304L SS inS_u 'fatedJ- 13 Water at 9_'_C................................................................................................... 4 3
40 Nominal Stress versus Plastic Strain for Incoloy 825 in SimulatedJ--13 Water at 93_ .......................................................................................................................... 44
4 1 Variation of Stress Ratio versus Plast.lc Strain for Incoloy 825 inSlm_dated J- 13 Water at 93°C .................................................................................................... 4 4
42 Nominal Stress versus Plastic Strain for Cu-7Al in Simulated J-.13Wat_ at _Y_ .................................................................................................................................... 45
1|! v||!
![Page 5: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/5.jpg)
43 Variation of Stress Ratio versus Plastic Strain for Cu-30Ni in SimulatedJ-13 Water at 93_ ......................................................................................................................... 45
44 Comparison of Stress Versus Plastic Strain for Two Tests on Type304L SS in Simulated J-13 Water at 93°C ............................................................................ 46
4 5 Comparison of Stress Versus Plastic Strain for Two Tests oll Type316L SS in Simulated J-13 Water at 93°C ............................................................................ 46
,16 Comparison of Stress Versus Plastic Strain for Two Tests on Incoloy825 in Simulated J--13 Water at 93°C ...................................................................................... 4 7
47 Comparison of Stress Versus Plastic Strain for Two Tests on Cu-30NIin Simulated J-13 Water at 93_ ............................................................................................... 4 7
48 Compazlson of Stress Versus Plastic Stlain for Two Tests on Cu-7AI inSimulated J-13 Water at 93°C .................................................................................................... 48
49 Relative Cracking Susceptibility of Five Alloys in Simulated J-13Water at 93°C, Expressed in Terms of Nominal Stress Ratio ....................................... 4 9
50 Relative Cracking Susceptibility of Five Alloys in Simulated j.-13Water at 93°C, Eacpressed in Terms of Nominal Strain Ratio ........................................ 4 9
51 Cracking Susceptibility of Incoloy 825 and Cu-30Ni in Terms of StressRatio or Strain Ratio in j-13 Water at 93°C ......................................................................... 5 0
52 Relative Cracking Susceptibility of Five Alloys in Simulated J-13 Waterat 93°C, Expressed in Terms of Nominal Stress Ratio ..................................................... 50
53 Relative Cracking Susceptibility of Five Alloys in Simulated j-13 Waterat ,q3°C, Expressed in Terms of Nominal Strain Ratio ..................................................... 5 I
54 Electrochemical Potential of Incoloy 825 and Cu-7%Al Alloy SSRTSpecimens at 93°C versus an Extenml Reference Electrode as a Functionoi"T_e during Tests W- 13 and W- 15 ................................................................................... 5 8
55 Potential for Converting ECP Measurements from an Ex_enaal Silver ChlorideReference Scale as a Function of the KCI Concentration fromRelations for Thermocell and Liquid Junction Potentials .............................................. 60
56 Influence of Temperature o.n the Potential for Converting ECP Measurementswith an External Reference Electrode to the Standard Hydrogen Electrodefrom Relations for Thermocell and Liquid Junction Potentials ................................... 60
57 Design of Compact Tension Crack-Growth-Rate Test Specimen ............................... 63
58 Schematic Representation of Experimental Setup and Test Specimen ................... 65
59 Crack Length vs. 'rest Time for Type 304L SS at Kmax = 25 MPa.m I/2and R=0.9 ......................................................................................................................................... 68
60 Crack Length vs. Test Time for Type 316L SS at Kmax .= 25 MPa.m I/2 andR=0.9 .................................................................................................................................................. 68
61 Crack Length vs. Test Time for Incoloy 825 at Kmax = 25 MPa.m I12 andR= 0.9 ................................................................................................................................................. 69
62 Crack Length vs. Test Time for 304L SS at Kmax = 36 MPa.m I/2, R =0.7 and 0.5 l-Lz................................................................................................................................... 69
![Page 6: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/6.jpg)
63 Time-Based CGR vs. Rate for Austenitic Stainless Steels in Air fromASME Section XI Correlation ibr R -- 0.5 .............................................................................. 70
64 T_ne--Based CGR vs. Rate for Austenitic Stainless Steels In Air fromASME Section XI Correlation for R = 0.7 .............................................................................. 70
65 Th_e--Ba.,_d CGR vs. Frequency at R = 0.5 ............................................................................ 71
66 "rlme-_ CGRvs. l,h'equency at R = 0.7 ............................................................................ 71
67 CGR per Cycle as a Function of Rise Time for R = 0.5 ..................................................... 72
68 CGR per Cycle as a Function of Rise Tnne for R = 0.7 ..................................................... 72
I
i| viii
||
![Page 7: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/7.jpg)
Tables- -- -- li=.r ..... _ _ i i__ .
1 F_em_ntalC(xnposiUonof Well J- 13 Groundwater .............................................................. 3
2 Elemental Composition of Type 304L Stainless Steel Base Metal andType 308L Stainless SteelWeld FtUerMetal........................................................................... 5
3 Elemental Composition of Type 316L Stainless Steel Base Metal andType 316L StainlessSteelWeld Filler Meta].......................................................................... 5
4 Elemental Composition of Incoloy 825 Base Metal and Inconel 625and Inconel 65 Weld Filler M_ml................................................................................................ 6
5 Elemental Composition of Phosphorus-Deoxldlzed Copper .............................................. 6
6 Elemental Composition of the Cu-30%Ni Alloy and Monel 67 WeldFillerMetak ................................. .......................................................................................................... 7
7 Elemental Composition of the Aluminum Bronze Base Metal Alloysand Specifications for the Aluminum Bronze A2 Weld Filler Metal ............................... 7
8 Selected Mechanical Properties of the E_perimental Materials .................................... 8
9 Yield Stress of Smooth Base and Welded Candidate Waste Container
I 0 Summaly of Experimental CondIUons fox"SSRT Tests ....................................................... 9
I I SSRT Results for Candidate Container Materials in Simulated J-13Water at 93_ ....................................................................................................................................... 14
12 SSRT Results for Candidate Container Materials in Simulated J-13Water at 93_ ........................................................................................................................................ 14
13 ,%.¢_RTResults on Weldment Specimens of Candidate Container MaterialsIn Slmulated J.-13 Water at 93"C.................................................................................................. 15
14 SEM Observations on SSRT Specimens of Candidate Waste ContainerBase Materials Tested in Simu 'lated J- 13 Water at 93°C .................................................... 16
15 SEM Observations on SSRT Specimens of Candidate Waste ContainerWeldment Specimens Tested in Simulated J- 13 Water at 93°C ..................................... 17
16 SSRTs on Waste Container Materials at a Strain Rate of 1 x 10.7 s"I inS_ulated J- 13 Water at 93°(3....................................................................................................... 3 7
17 Chemical Composition of Effluent Water from SSR'Fs on Cm_didateWaste Container Materials, Tests W- 1 through W-9 ............................................................. 52
18 Chemical Composition of Effluent Water from SSRTs on CandidateWaste Container Materials, Tests W- I0 through W- 18 ....................................................... 53
19 Chemical Composition of Effluent Water from SSRTs on CandidateWaste Container Materials, Tests W-19 through W-27 ........................................................ 54
20 Chemical Composition of Effluent Water from SSRTs on CandidateWaste Container Materials, Tests W-28 through W-33 ....................................................... 5 5
2 1 pH25oc of Effluent Water and pH93oc in Vessel during SSRTs inSimulated J- 13 Water ....................................................................................................................... 5 8
_I viii
![Page 8: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/8.jpg)
22 Steady-State Electrochemical Potential of Candidate Waste ContainerMaterials, Platinum, and Nickel Test Vessel during SSRTs inSh-nulated J- 13 Water at 93_C....................................................................................................... 59
23 ChernOff Composition of J-13 Well Water and Test Solution .......................................... 62
24 Loading Conditions for CGR Tests on Candidate Waste Container--************************************************************************************************************************************************ 64
25 C'yclic CGRs, Observed and Calculated with ASME Section XI Correlation ................. 67
![Page 9: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/9.jpg)
STRESS CORROSION CRACKING OF CANDIDATE
WASTE CONTAINER MATERIALS - FINAL REPORT
by
J. Y, Park, P. S, Mary., W. K. Soppet, D, R. Die.ks,W. J. Shack, and T. F. Kassner
Abstract
Six alloys have been selected as candidate container materials for the storage of high-level nuclear waste at the proposed Yucca Mountain site in Nevada. These materials are
Type 304L stainless steel (SS), Type 316L SS, Incoloy 825, phosphorus-deoxidhT.ed Cu, Cu-30%Ni, and Cu-7%Al. The present program has been initiated to determine whether anyof these materials can survive for 300 years in the site environment without developingthrough-wall stress corrosion cracks, and to assess the relative resistance of thesematerials to stress corrosion cracking (SCC). A series of slow-straln-rate tests (SSRTs) andfracture--mechanics crack-growth-rate (CGR) tests was performed at 93°C and 1 atm ofpressure in simulated J-13 well water. This water is representative, prior to the
widespread availability of unsaturated-zone water', of the groundwater present at the YuccaMountain site.
Slow-strain-rate tests were conducted on 6.35-mm-dlameter cylindrical specimensat strain rates of 10 -7 and 10-8 s-l under crevice and noncrevice conditions. All tests were
interrupted after nominal elongation strain of 1-4%. Scanning electron microscopyrevealed some crack initiation in virtually all the materials, as well as weldments madefrom these materials. A stress- or straln-ratio cracking index ranks these materials, inorder of increa._ing resistance to SCC, as follows: Type 304 SS < Type 316L SS < Incoloy825 < Cu-30%Ni < Cu and Cu-7%Al.
Fracture-mechanics CGR tests were conducted on 25.4--mm-thick compact tension
specimens of Types 304L and 316L stainless steel (SS) and Incoloy 825. Crack-growthrates were measured under various load conditions: load ratios (]R)of 0.5-1.0, frequenciesof 10-3-1 Hz, rise times of 1-1000 s, and peak stress intensities of 25-40 MPa_ml/2. The ::measured CGRs are bounded by the predicted rates from the current ASME Section XIcorrelation for fatigue CGRs of austenitic stainless steel in air. Environmentally accelerated
crack gro;',-th was not evident in any of the three materials under the te3t conditionsinvestigated.
![Page 10: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/10.jpg)
1 Introduction
1.1 Objectives
The objectives of the present program are to (1) determine whether any of the six
candidate alloys currently under consideration as waste container materials can survive for300 years in the Yucca Mountain repository without developing through-w_ll stresscorrosion cracks, and (2) rank the candidate materials in terms of their re,_istance to
stress corrosion cracking (SCC) in the repository environment. Two types of tests wereconducted: (1)slow-strain-rate tests (SSRTs), and (2)crack-growth-rate (eGR) tests basedon standard compact tension (CT) fracture-mechanics specimens. In the overall test
program, approximately 33 SSRTs were performed on six candidate materials, togetherwith eGR tests on six CT specimens from three candidate materials in simulated wasterepository groundwater. This is the final report for the program.
1.2 Background
In December 1987, Congress amended the Nuclear Waste Policy Act of 1982 anddesignated the Yu_._a Mountain site in southern Nevada as the nation's first high-levelnuclear waste repository, if further investigations confiral that it is suitable. YuccaMountain is located on the southwestern boundary of the Nevada Test Site, and thegeologic horizon at the proposed location for the repository is compacted volcanic ash, ortuff, consisting of quartz, chrlstobalite, alkali feldspar, and other minor phases I situatedabove the permanent water table. Thus, interaction between groundwater and the wastepackages should be minimal.
The high-level waste packages consist of three major components: the metalliccontainment barriers (the containers or canisters), the waste itself, and other materials,
including packing materials, emplacement-hole liners, etc. The metallic containers areintended to provide essentially complete containment of the nuclear waste for 300 to
1,000 years after emplacement. During the waste isolation or postcontainment period thatextends for thousands of years after the metallic containment barriers are breached, thewaste itself is expected to control the pate of release of radioactive nuclides into the
immediate repository environment. The temperature of the waste package will besufficiently high for much of the time so that the limited groundwater in the vicinity of thepackage will be present only in the form of steam. Nonetheless, the proposed tests willfocus on aqueous environments at _.93°C, because these environments are expected to
provide deleterious conditions (which may provide the "worst case") for SCC susceptibility.The elemental composition of Well J-13 groundwater, which is representative of the
groundwater present at the Yucca Mountain site, is summarized In Table 1.2
2 Test Materialsiii ........ tr.-.. -
Six candidate materials are being tested, namely Type 304L stainless steel (SS), Type316L SS, Incoloy 825, P-deoxidlzed Cu (CDA-122), Cu-30%Ni (CDA-715), and Cu-7%Al (Al
bronze, or CDA-614). 3 These materials were chosen as candiaates because of their goodcorrosion properties and their extensive use in the marine, nuclear, and processindustrles. 4 The alloys were obtained from Lawrence Livermore National Laboratory (LLNL)in the annealed condition.
![Page 11: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/11.jpg)
Table 1. Elemental Composition of Well J-13 Groundwater a
w..
Concentration ConcentrationElement (mg. L- !) Anion (rag. L- !)
Ca 11.75 p-I 2.1
Mg 1.76 CI-I 6.4
Na 45.0 SO2 18. I
K 5.3 HCO3 143.0
Li 0.06 NO3 10.1
Fe 0.04 - -
Mn 0.001 -- -
Al 0.03 - -
SI 30.0 - "-
aDissolved oxygen concentration, 5.7 ppm; pH, 6.9
The following weldments, fabricated from these base materials by LLNL, are alsobeing tested (the second alloy indicated in each pair is the weld filler metal): Type 304LSS/308L SS, Type 316L SS/316L SS, Incoloy 825/Incoloy 65, Incoloy 825/Inconel 625,Cu-30Ni/Monel 67, and Cu-7AI/AI bronze A2. The weldments were made by the gas-metal-
arc welding (GMAW) process. In addition, LLNL supplied Cu and Cu-7AI weldments
produced by the electron-beam welding (EBW) process. These latter weldments wereproduced without filler metal, and the fusion zones are narrow compared with the GMAWweldments.
Elemental compositions of the base and weld filler metals are given in Tables 2-7,and selected mechanical properties provided by vendors are given in Table 8. The yield
strengths of the base materials and weldments were determined independently by
Argonne National Laboratory at room temperature and at 93°C. and these values arepresented in Table 9.
3 Slow-Strain-Rate Tensile Tests
3,1 ExperimentalProcedures
Fabrication drawings for the SSRT specimens are shown in Figs. 1-3, and thelocations of welds in the GMAW and EBW specimens are shown in Figs. 2 and 3,
respectively. Similar specimens were used in our earlier studies on SCC of austeniticstainless steels in simulated boiling w_ter environments. 5,6 The small-diameter {=0.8-0.9
mm) through-holes localize the strain and cracking, thereby facilitating observation of SCC
|
![Page 12: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/12.jpg)
by scanning electron microscopy (SEM). When pins of matching materials are inserted inthe holes, crevices are produced.
The SSRTs were conducted in simulated J-13 water at 93°C at strain rates of 10 -7
and 10-8 s-I for the base specimens and were interrupted after elongation (plastic) strainsbetween 1 and 4%. The tests were conducted in a 1.270--L Ni container. A worm-gear
Jactuator, gear reducer, and a variable-speed control system were used to apply the strain.The temperature was maintained by clamp-on heaters with associated instrumentation. A
once-through water system with a flow rate of =3 mL/min was used. The SSRT system,including the feedwater system and the electrochemical-potential (ECP) monitoring
system, is shov, n in Fig. 4.
For tests W-1 through W-23_ the flow of simulated J-13 water was maintained by anoverpressure in the feedwater tank and the flow rate was controlled by a capillary tubeconnecting the feedwater tank to the test chamber. After a number of tests, the capillarytube was found to be clogged by the insoluble silicon compounds and bicarbonates.Therefore in tests W-23/W-33, a mechanical peristaltic pump was installed in thefeedwater line to ensure a more continuous flow through the environmental chamber.Also, the water chemistry for the early tests was varied from test to test as varioussimulations of J-13 water were examined, to avoid excessive formation of precipitates at
the test temperature. Details of the simulated J-13 water chemistry, its characterization,and the procedures for measuring ECP are described in a subsequent section of this report.
For tests W-13/W-33, a dial indicator was connected to the Jactuator to measure the
displacement of the pull rod. This measurement, along with measurements of the systemcompliance, can be used to estimate the strains in the specimen during the test.Measurements of the total specimen length before and after the tests give even moreaccurate values of the actual elongation (plastic strain). After each test, the specimen was
sectioned by electrical-discharge machining (EDM), as shown in Fig. 5, so that the entirehole region could be examined by SEM at magnifications up to 2000x to detect stresscorrosion cracks. 6
In tests W-1 through W-7, pins of a matching material were inserted in the twothrough-holes to produce crevices. The tests were conducted at a strain rate of 10-7 s 1and were interrupted after elongations of 3-3.7%. During the tests, the top crevice wasexposed alternately to water and vapor, and the bottom crevice was kept immersed inwater. Siphon action in the inverted drain tube shown in Fig. 4 exposes the top crevice toalternate liquid and vapor. The bottom crevice is always immersed in liquid. 'When thehole at the top of the drain tube is opened to the atmosphere, both crevices can be
exposed to liquid only.
Tests were also performed on the base materials at a strain rate of 10-8 s -l toinvestigate the effect of strain rate on SCC. In these tests, one of the holes was left open,but a pin was inserted in the other to produce a crevice. The entire specimen wascontinuously exposed to the liquid. These changes were made to determine whether acrevice is necessary for cracking of the materials. The tests were interrupted after plasticelongations or strains of _ 1.0--1.6%, which are somewhat lower than the strains at whichthe tests were internJpted at the higher strain rate, Welded spectmcns were strained at a
i i
![Page 13: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/13.jpg)
5
Table 2. Elemental Cornr_sltton (wt.%] of Type 304L
Siainless Base Meta[ a'nd '_ipe 308L Staln[essSteel Weld Filler Metala
._.I_..._.O4L a.LE]£s_s Steel Type .'_SL SS,}-[eat V?020(I ____ Heal '_!70_.q_312 Heat K6835
Element Vendor Vcmdor Independent Vend_r
C 0.023 0.015 0,02 O.0l 9
Mn 1,79 1,82 I,_9 2,22
P 0.03 0,03 0,024 0.015
S 0_C l@ 0.018 0,016 O.O01
Si O.;_J 0.4 0.34 0.37
Cr 18.15 18.21 19.09 19.6
NI 8,25 8,16 Li,.73 9,53
CU 0.26 0,3 0,3 0. I
Mo 0.3 0,34 0,26 0.07
Co 0,14 0,15 - -
N 0,079 0.093 0.095 -
O .... 0.009
a Vendors were F.._stenl Stafnl,e_,a Steel Company for the Type 304L SSand American We_d(ng Al_oy_ for the. Type 308L SS. The indepe|_dentanalysis was F_ffon'rke.d by An,ap_'t [.aboratork::s, Inc.
Table 3. Eleme.ntal Composlt_on (wt,%} of Type316L Stainless Steel Base Metal (Heat
16650) and T_pe 316L Stainless Steel
Weld F'iller Metal (Heat 4H3367)a
_ Hteat 18_,_..____ Heat 41[3367Element Vendor Independeut Vendor
C 0.018 0.018 0,018
Mn 1,78 l,SG 1.98
P 0,026 0.022 0.023
S 0,013 0.016 O.018
Sl 0,_3 0,40 0.63
Ct 16,5 i6.84 18,69
NI IO.3'_J I 1. I 12.2'9
" Mo 2.09 2. I -o
Cu O,19 O.17 0.25
di Co 0.1 - -
N C.054 0,058 -
0 - 0.0[0 -
J'_%'end,or_were ,J(.,_._)p Sl('(-I C(m_I_,_hy[or _h_' ha.,,(' n_clal
* and Arm'n,c'an Wc_dl_ Ali())'.,, I_}r t l_' 'l'Vpc. 3081. SS. '}'heai
l:r_depe:r_cle:ntan,alyst,,_wa,_ l_:do,rn'_-"d by Aname,lLabomto,r_ea, l_c.
|,
![Page 14: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/14.jpg)
"Fable 4. Elemental Cornpositton (wt.%) ,rf Incoloy 825 Base Metal and
Inconel 625 and lncotoy 65 Wetd Filler Metal a
Incoloy 825 , Inconel 625 Incoloy 65"---Heat-- Heat Heat Heat_._H2,__!12__5F-.-_ HH3884FG _:_ VX0451AY N50ABH
Element Vendor Vendor Indep't Vendor Vendor
C 0.02 0.01 0.014 0.04 0.041
Mn 0.39 0.46 0.47 0.07 0.43
Fe 27.98 27.4 balance 4.2 28.79
S 0.003 0.001 0.004 0.001 0.001
Si 0.14 0..31 0.33 0.19 0.18
Cu 2.03 2.06 1.98 0.1.0 l.Sx
Ni 43.89 43.55 43.5 60.03 42.83
Cr 21.98 22.11 22.44 22.21 22.21
AI 0.03 0.06 0.06 0.24 0.09
Ti 0.75 0.83 0.84 0.27 0.91
Mo 2.79 3.21 3.12 9.06 2.72
Cb+Ta - 0.36 3.58 - -
N - 0.007 - - -
O - 0.0.04 ....
P - -- 0.010 0.017 --
a Vendor was INCO Alloys International for ali of these alloys. Theindependent analysis was performed by Anamet Imboratories, Inc.
Table 5. Elemental Composition (wt.%) qf Phosphorus-Deoxldtzed Copper a
Heat 7374 Heat 6653
Element Analysis 1 Analysis 2 Analysis i Ana_ysls 2 Independent
Cu 99.90 99.90 99.9.0 99.90 99.95
P 0.039 0.039 0.027 0.030 0.032
a Vendor was Revere Copper Products, Inc.. for bob heats of material; twoanalyses were provided with each heat. The Ind:ependent analysis wasperformed by Anamet Laboratories. Inc.
![Page 15: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/15.jpg)
7
" NTable 6. Elemental Composition (wt.%) of the Cu-30% i Alloy
and Monel _7 Weld Filler Metal a
, Jl,
Cu-30%NI Monel 67Heat 673 Heat 050 Heat N5GABH
Element Vendor Analysis l Analysls2 Independent Vendori
O.1 69.52 69, '73 67.96 68. I 68.51
Ni 29,4 29.3 31.0 30.7 29.72
Pb 0.004 0.006 0,005 <0.005 <0.001
Fe 0.55 0.52 0.59 0.50 0.50
Zn O.03 0.03 0.03 0.09 -
P 0,O01 0.001 0,001 <0.005 0.008
Mn 0,44 0.43 0,41 0.51 0.81
C 0.011 0.008 0.008 0.03 -
S 0.002 0.001 0.002 <0.005 0.001
SR ...... 0.I
Ti ..... 0,35
a Vendor was Hussey Copper, Ltd,, for both heats of base (two analyseswere provided for I-l[eat 050]. ]NCO Alloys International was the vendorof the Monel 67 weld filler meta|. The independent analysis wasperformed by Anamet Laborato_es, Inc.
Table. 7. Elemental Composition (wt.%) of the Aluminum Bronze
Base Metal Alloys and Spec_Ications.for the AluminumBronze A2 Weld Filler Metal a
Aluminum Bronze Al Bronze A2
Heat 5485 Heat 5263-A HeatAna_y- Analy- Anabr- Analy- Indepen-K9KO2298A
Element. sis 1 sls 2 sls 1 sis 2 (tent Vendor
O.1 90.69 9J, 76 9'0,67 90.52 balance balance
Al 6.64 6.65 6.55 6.49 6.19 9.0--I 1.0
Fe 2.41 2.23 2,42 2.63 2.97 <I ,5
P 0.001 0.001 - - <0.005 -
Zn - - 0.26 0,25 O.14 _<0.02
Mn ...... 0,09
Pb ..... _0.02,,,,,, , i• .t L , N,.
a Vendor was WiIILams & Company, Inc., for both heats of base melal {twoanalyses were p rovillded fo,r each heat]; J. W. Harris Co., was the vendorfor the weld metal (Heat K9K02298AI. The independe.nt analysis wasperformed by Anamet Labo,rator_eso lhc,
=m
![Page 16: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/16.jpg)
8
Table 8, Selected Mechanical Properties of the ExperimentalMaterials a
Yield Tensile Total Reduction
Material and Strength Strength Elongation of AreaHeat No. (MPa) (MPa) (%} (%) Hardness
Type_04L SSV70200 273 594 59 66 HB 156
V70312 292 614 55 64 HB 160
Type 316L SS16650 231 530 53.9 72.0 BIIN 137
Incoloy 825
HH2125F 298 676 43 62 RB 85
HH3884FG 321 712 47 69 RB 8,'I
Copper
6653 - 232 55-59 - F6 l
7374 - 220 - -
Cu.-30% Ni
050 177 388 45.5 - RB 42-48
673 1 77 366 44-45 - RB 64--65
aMechantcal properties provided by the vendors.
Table 9. Yield Stress of Smooth Base a and Welded bCandidate Waste Container Materials
}{eat Number Yield StressMaterial Base/Weld Base Weldment {Ksi}[MPa]
304L SS V70200 x - (40.5) [279]
316L SS 16650 x - (37.3} [257]
Incoloy 825 H2125F x - {50.5) [3481
Oi 7374 x - (l 1.4) [79]
Cu-7%Al M5485 x - (44.6) J307]
Cu-30%Ni 673 x - (23.8) [1641
304L SS V70312/WO04 - x (52.8) [364]
316L SS 16650/W002 - x (48.8} [3361
Incoloy 825 HH3884FG/WOI0 - x (55.3) 381]
Incoloy 825 HH3884FG/W007 - x (55.3) 381]
Cu e 6653/6653 - x (19.5) 1341
Cu-7q_l M5263A/W014 - x (44.9) 3091
Cu-7%AI M5263A/M5263A - x (44.9) 309]
Cu-30%Ni HFO50/WOI 3 - x (23.8) 164]
= Tensile tests on unwelded specimens were performed in air at ix)ore
temperature, at a strain rate of 2.2 x 10 "4 s "'I.
b Tensile tests on weldments were performed in air at 93_C at the samestra!n rate as u.._'d for ba._c materials. Yield stress for _he wcldnx'nt(snx_oth) specimens arc estimated from the yield ,_tress determinedfor the srr_oti_ specimens with holes, taking into acctmnt the reducedcross section due to the hole.
Thence weldments were produced by electron-beam welding; all the
---i other weldments were made by gats-ri_=L-_ ........ es.
i=¢,,
![Page 17: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/17.jpg)
Table l O. Summary of Experimental Conditions in SSRT Tests
Pull Rod Strain at Si Level HCO3 LevelTest Flow Dial Exposure Interrupt In Water In Water
Nurnber Control Indicator Conditions a (%) (ppm) (ppm)
Base Metal Tests at t = lO-7 s-1
W- 1 overpressure no 1 4.9 530 622W-2 overpressure no 1 3.0 30.2 78.0W-3 overpressure no 1 3.4 29.4 44.0W-4 overpre ssu re no 1 3.7 29.6 36.0W-5 overpressure no 1 3.7 27.6 15.0W-6 overpressure no 1 3.6 29.1 25.0W-7 overpressu re no I 2.9 29,2 19.0W- 12b overpressure no l 3. I <0. I 128.0
Base Metal Tests at t = 10-s s"I
W- 13 overpressure yes 4 1.2 137.0W- 14 overpressure yes 4 1.3 - 125.0W- 15 overpressure yes 4 1.0 - 130.0W- 18 overpressu re yes 4 1.5 - 131.0W- 19 overpressure yes 4 1.6 - 134.0W-20 overpressu re yes 4 1.6 - 134.0
Weldment Tests (t = 10-7 s "l)
W-9 overpressure no 3 2.3 0.18 52.0W- 10 overpressure no 3 2.7 0.13 128.0W- l I overpressu re no 2 2.9 <0. I 133.0W- 16 overpressure yes 3 2.8 133.0W- 17 overpressure yes 3 3.0 133.0W-21 overpressure yes 2 3.2 133.0W-22 overpressure yes 3 3. I 130.0
Supplemental Base Metal Tests (t = 10 "7 s -l)
W-23 pump yes 2 26.6 e 133.0W-24 pump yes 2 18.2 137.0W-26 pump yes 2 5.6 139.0W-27 pump yes 2 6, I - 142.0W-28 pump yes 2 5.0 - 141.0W-29 pump yes 2 5.5 - 140.0W-30 pump yes 2 5.7 - 138.0W-31 pump yes 2 5.6 - 135.0W-32 pump yes 2 I 1.93 - 134.0W-33 pump yes 2 I 1.88 - 134.0
Supplemental Weldment Test (t = 10 "7 s -I)
W-25 pump yes 2 3.2 - 141.0
al = two holes, two pins: one hole exposed continuously to liquid; the other alternately to liquidand vapor.
2 = two holes, two pins: both holes exposed continuously to liquid.3 = three holes, three pins: all holes exposed continuously to liquid.4 = two holes, one pin: both holes exposed continuously to liquid.
b Repeat of invalid test W-8.
c Test run to failure.
l
![Page 18: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/18.jpg)
10
L 76.2O ,_
I 6,35 DIA.
__ ....__._?__......LB.__.,,o,_.
-- 19.05 --_
\.,,jTWOTHROUGHHOLES 0.8 TO 0.9
Fig. I. Fabrication Drawing for Base Metal SSRT
Specimen. Dimensions are in mm,
i 76.20 _-
6.35 DIA. /
,,/ ' -- LOCALE EDGE OF THIS, 0.8TO O.9THROL_H IE)LE\ APPROX. 0.4 FROM WELD
"-- __.,_u_ L-- o._,oo.__._o_..o_IN CENTER OF WELD
F_g. 2. Fabrication Drawing for Gas-Metal-Arc Welded
Specimen. Dimensions are in mm.
i
![Page 19: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/19.jpg)
II
I ;6.20 ..........6.35 DIA. I
----:- ] ,1, ..........---
L-_,/ /1' -,,,--"--",,F_.=__----.____,.__
/ _--- LOCATE EDGE OF Tills
_- O.BTO 0.9THROUGH HOLE
Fig. 3, Fabrication Drawing for Electron-Beam-Welded
Specimen. Dimensions are in mm.
TEFLC:, INSLJLATEDPLAT,NbM WiRE
LOW PRESSURERE_UL.ATOR
E- -]_..(" VENT I f_--/i/ROOM TE_,'.°
....... I // I lr ELECTRC_E
,o,,,RAII G_I I I I ..M,xEOOAS II_ -_'--- 4--._T°0
laiii I I j/ 8ueSL_R _ -,,_ j -\.HEATER ""
, ,jSL',F\L__ SEA \
1 NICKEL TESTCHAMeERI
oE_Eo--:l _ _ _ ox,o,zEoZR7c5
WATERCHEMISTRYSAMPLING POINT
Fig. 4. Schematic of SSRT Setup with Feedwater and
Electrochemical Potential Monitoring Systems,
![Page 20: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/20.jpg)
12
Fig, 5_ Cross-Sectlonal View ofDrilled Hole in SSRT
Specimen
rate of 10 -7 s'l and IntexTupted after elongations of 2.3-3.2%. In the tests on weldspecimens, all of the crevices were continuously immersed in water.
lt should be pointed out that in the series of tests conducted at the two strain rates,
namely, 10 -7 and 10-8 s-I, different exposure conditions were used. In the testsconducted at the faster strain rate (tests W-1/W-7), pins were inserted in both holes of
the specimen (two c-evlces). Only one of the holes was exposed continuously to liquid; theother was exposed alternately to liquid and vapor phases. In addition, the water chemistryfor the first test (W-l) was vastly different from the rest of the tests. In the testsconducted at the slower strain rate of 10-8 s -l, the water chemistry is not comparable tothat used for the tests conducted at the faster strain rates. Also, in the slower strain rate
tests, only one of the holes was left open (noncrevice), and a pin was inserted in the other
to produce a crevice. Both holes were continuously exposed to simulated J-13 water.Because of these differences in test conditions, the strain-rate effects observed in this
work should be regarded as very preliminary.
The varying experimental conditions for the SSRT tests are summarized in Table I0.These differences should be borne in mind when reviewing the test results.
3.2 SSRT Results (Tests W-I/W-22)
3.2.1 Observations of SCC by SEM
The SSRT results for the initial base metal tests are summarized in Tables 11 and 12
for the weldment tests in Table 13. The SEM observations for all the tests conducted at a
strain rate of 10-7 s -I are summ.artT.ed in Tables 14 and 15. The results of the initial basemetal and weldment tests show some cracking in virtually all the specimens, includingthose tested at the slower strain rate of 10- 8 s-l. However, in most cases, crack
![Page 21: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/21.jpg)
13
observations were made at magnifications as high as 1000-2000x, because it was difficultto observe well-defined cracks at magnifications lower than lOOx. Hence, the actual crack
depths inferred from the size of the crack opening are _mall (in the micron range) evenfor Type 304L SS. These findings are consistent with our unsuccessful efforts thus far to
observe cracks >10--20 _tm in depth in the transverse metallographic specimens of Type304L SS. The cracks in Type 304L SS are more open (and hence are probably deeper)than those in Incoloy 825, as shown in Fig. 6. This is consistent with the expectedincreased resistance of Incoloy 825 to SCC because of its higher Ni content. However.Incoloy 825 shows a larger number of cracks than Type 304 SS.
The cracks in Incoloy 825, which appear to have initiated at machining marks thatare favorably oriented for cracking, appear as thin straight lines in Figs. 6 and 7. lt is notclear whether the larger number of cracks in the Incoloy 825 is due to the machiningmarks. Such straight marks are also frequently seen in specimens of other' materials,although they were not observed in our earlier studles on SCC of austenitic stainless
steels, s,e These machining marks are attributed to the use oi'a slightly modified drillingprocedure that was adopted 'after completing 25 tests. However, this change in procedurewas not found to affect the stress/strain response of the materials in the simulated J-13water environment.
For the Ivcoloy 825 weldment, where the base metal is a different heat, poor surfacefinish made it difficult to determine whether cracks were present in the base metal, as
shown in Figs° 7a and 7c. The filler material, however, showed pronounced cracking (Fig.7b).
Scanning electron microscopy of the Cu and Cu-base alloy spcclmens reveals thatthese materials also showed some signs of cracking in simulated J-13 water. As shown inFig. 8, there is no discernible difference in cracking among the three Cu-based materials.
Cracking in Cu (Fig. 8a) and in Cu-301,_i (Fig. 8c) occurred both at the mac:,ining marks(which are nearly straight) and elsewhere (cracks with wavy appearance). On the basis ofthese observations, it appears that the differences in SCC susceptibility of the three Cu-based materials are small compared to those, for example, between Type 304L SS and
Incoloy 825. Further quantification oi' SCC in terms of crack depth and growth rate isrequired to better delineate differences in cracking behavior.
Cracking has also been observed in all the weldments tested. For example, the Type316L SS weldment with matching filler metal shows cracking both in the weld and basematerial (Fig. 9). The Cu-3ONi weldment specimen also exhibited cracking, and there wasno clear--cut difference in the appearance of cracks in the base, weld, and heat-_,d'fectedzone (Fig. I0).
The cracking behavior of the crevices continuously exposed to liquid was not muchdifferent from that of crevices alternately exposed to liquid and vapor during the tests.This is illustrated in Fig. 11 for an Incoloy 825 specimen, lt also appears that a crevice isnot required for SCC to occur in these materials. As shown in Fig. 12. the cracking at
holes with and without pins appears similar for Incoloy 825 and Cu-3ONi. On the basis ofSEM observations, it is also difficult to determine whether the change in strain rate had
any effect on cr"acking, because the observed differences are small and the tests performed
II,relr' ' 'lqF, ¢lFIn'q,rl" 'lllP"' Ill' ' vln III nr * eplIlr 'U q''r ...... i li]lr '11'11'p'_ q_ll1''F1 ,nn 'IHP Inr, . InP_lnp,_rVll"ll _ ' ,rllq_Fn_llI ,rn;lllll_l '
![Page 22: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/22.jpg)
14
Table 1 I. SSRT Results for Candidate Container Materials (two holes with
pins inserted in each) at a Strain Rate of 10 -7 s -I irl SimulatedJ-.l 3 Water at 93 °C
Specimen Local Nominal NominalTest Heat ECP, Elongation Strain a Stress StrainNumber Material Number (mV[SHE]) _:p (%) (%) Ratio b RatloC
Wl IN 825 H2125F 233 4.9 15.1 0.93 0.82
W2 IN 825 H2125F 253 3.0 8.1 0.94 0.83
W3 Cu-30Ni 673 - 3.4 9.0 0.96 0.87
W4 304L V70200 310 3.7 d 0.80 O. 19
W5 Cu 7374 303 3.7 15.2 0.99 1.00
W6 316L 16650 268 3.6 d 0.81 0.5 l
W7 Cu-6Al M5485 323 2.9 8.6 1.00 1.07
Wf2 O.1 7374 308 3. I I0. I 0.91 0.78
aThe local strain is computed as the product of a strain concentration factor I_,estimated from Neuber's rule, and the nominal strain in the unreduced gaugesection, which is determined from the stress-strain curve and the measured loadon the specimen. Kr depends on the material and strain level.
bSee Eq, 13.
cSee F_xi.17.
dToo low to estimate accurately.
Table 12. SSRT Results for Candidate Container Materials (two holes, one with
a pin and one withouO at a Strain Rate of 10 -8 s"-I in SimulatedJ- 13 Water at 93 °C
Specimen Local Nominal NominalTest Heat ECP, Elongation Strain a Stress StrainNumber Material Number {mV[SHE]) (%) (%} Ratio b Ratlo c
Wf3 IN 825 H2125F 383 1.2 d 0.87 0.40
Wl4 Cu-30Ni 673 293 1.3 2.3 0.97 0.88
Wf5 Cu--6Al M5485 268 1.0 4.5 1.01 I. 15
W18 Cu 7374 273 1.5 4.4 0.75 0.83
Wf9 3161, 16650 374 1.6 d 0.72 O. 15
W20 304L V70200 343 1.6 d 0.52
a The local strain is computed as the product of a strain concentration factor Ke,estimated from Neuber's rule, and the nominal strain in the unreduced gauge section,which is determined from the stress-strain curve and the measured load on thespecimen. Ke depends on the material and strain level.
b See Eq. 13.
c See Eq. 17.
d Too low to measure accurately.
o,i
![Page 23: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/23.jpg)
15
Table 13. SSRT Results on Weldment Specimens of Candidate Container
Ma...rials at a Strain Rate of 10 -7 s -I in Simulated J-13 Waterat 93°C
ID a Number Specimen _ NominalTest Base ECP Elongation StressNumber Material Weld (mV[SH El) (% ) Ratio b
W-9 Incoloy HH3884FG 290 2.3 0.95825 W010
W- 11 Cu 6653 2a3 2.9 0.89W019
i
W-lO Cu-3ONi HF050 238 2.7 0.91
W- 17 316L 16650 363 3.0 0.98WOO2
W-16 Cu-7A1 5263-A 294 2.8 1.2W014
W-21 Cu-7AI 5263-A 241 3.2 1.2_W020
W-22 Incoloy H3884FG 316 3. I 1. i82 5 WOO7
W-25 304L V70200 334 3.2 0.97WOO4
aiD=Identification; Base and weld materials are identified by heat numberand weld number, respectively.
bSee Eq. 13.
o b 20__/.Lm,
Fig, 6. SEM Photomicrographs of Hole Regions (with
Pins) of (_ Type 304L SS, Interrupted after
Ep = 3.796, and (b) Incoloy 825 Interrupted
after Ep = 3.0% (_ = I x 10-7 s-I).
![Page 24: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/24.jpg)
16
Table 14. SEM Observations a on SSPT .Specimens b oJ Candidate WasteContainer Base Materials Tested in Simulated J-13 Waterat 93°(?,
CrackingTest No. Material Heat No. Location Observed
W1 Incoloy 825 H2125F Top yesBottom yes
W2 Incoloy 825 H2;25F Top yesBottom yes
W3 Cu-30% Ni 673 Top yesBottom yes
W4 304L SS V70200 Top yesBottom yes
W5 Cu 7374 Top yesBottom yes
W6 316L SS 16650 Top cBottom c
W7 Cu-6% Al M5485 Top yesBottom yes
W12 Cu 7374 Top yesBottom ves
a All tests were conducted at a strain rate of 10--7 s-I and interruptedafter nominal strains of 3--4%. SEM observations were made atmagnifications between lOOx and 2000x.
b The specimen has two holes with pins of the same material insertedinto them to produce tight crevices. The specimen was exposed toJ-13 water irl such a way that the top hole with the pin was alternatelyexposed to water in liquid and vapor phases, but the bottom hole wasalways immersed in J- 13 water.
c This specimen was pulled to failure in liquid nitrogen following theinterrupted test to determine the feasibility of determining the cracklength, but it was not possible to examine the extent of cracking onthe fracture surface.
at the slower strain rate 10-8 s-I were interrupted at lower strains than those performedat a strain rate of 10-7 s-I (see Tables II and 12).
3.2.2 Estimation of Local Plastic Strains
To _late the observed crack initiation and growth to plastic strain, it is necessary toestimate the local plastic strain at the hole. The local strain is computed as the product ofa strain concentration factor Ke, estimated from Neuber's rule, and the nominal strain in
the unreduced gage section, which is determined from the stress/strain curve and themeasured load on the specimen.
![Page 25: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/25.jpg)
17
Table 15. SEM Obtervations a on SSRT Specimens b of CandidateContainer Weldment Specimens Tested in SimulatedJ-13 Water at 93°C
CrackingTest No. Material Heat No. Location Observed
W9 Incoloy 825 HH3884FG HAZ yesIncoloy 65 Weld WO I0 Weld yes
HH3884FG Base no
W10 Cu-30%Ni HF050 HAZ yesWeld W013 Weld yes
HF050 Base yes
Wl I Of 6653 HAZ no6653 Base yes
W 16 Cu- 7%AI M5263A HAZ yesWeld W014 Weld yes
M5263A Base yes
W 17 316L SS 16650 HAZ yesWeld WOO2 Weld yes
16650 Base yes
W21 Cu-7%AI c M52 63A HAZ yesM5263A Weld yes
W22 Incoloy 825 HH3884FG HAZ yesInconel 625 Weld WOO7 Weld yes
HH3884FG Base yes
a Ali tests were conducted at a strain rate of 10 -7 S-I and interruptedafter nominal strains of 3-4%. SEM observations were made atmagnifications between 100x and 2000x.
b Except for the electron-beam-welded specimens, each specimenhad three holes located as shown in Fig. 2. Each hole had a pininserted into it. The electron-beam-welded specimen has two holeswith pins. The specimens were completely immersed in simulatedJ-13 water duilng testing.
c Electron-beam-welded.
Stress/straln data for these materials can be described by the frequently usedRamberg and Osgood equation 7
a la_"' (1}
where a and _ are the nominal stress and strain, respectively, E is the Young's modulus,and a and m are constants. Locally, near the hole, the stress and strain are then given by
i_U
![Page 26: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/26.jpg)
i
18
C 1.40 ,/zm
Fig. 7. SEM Photomicrographs of Hole Regions (with
Pins) of Welded Incoloy 825 Interrupted after
ep = 2.3%: (al Base, (b) Weld, and (c) Heat-Affected Zone (e = I x 10 -7 s -l)
K_r. = aKa + _( aKa _m (2)E _--E_ '
where Kt and I_ are the strain and stress concentration factors, respectively, S_bstitutionof Neuber's rule s
K2 (3)Kc = Ka
(where K Is the theoretical elastic stress concentration factor) In Eq. 2 gives
K2 .te__q_ + Komct Eem (4)K o Ee + Ep Ee+E p
]1
![Page 27: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/27.jpg)
19
Flg, 8. SEM Pho!orntcragraphs qf Cracks in Hole Regions(with Pins) of Cu and Cu-Base Alloys: (a) Cu
Interrupted qfter _p = 3.7%, (b) Cu-6%AIIntemLpted after _"'l_= 2.9%, and (c) Cu-30%Nt
Interrul_ted after t.'p = 3,4% K = I x 10''_ s-l),
_g. 9, SEM Ptmtomicrographs qf Cracks In Hole Regions(with Pins) of Welded Tljpe 316L SS Interrupted after
_p = 3,0%: (a) Base, and (b) Weld _ = 1 x i0 -'/ s-l).
![Page 28: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/28.jpg)
2:0
C 40/.Lm •
Fig. I Oo SEM Photomicrographs of Cracks in Hole Regions
(with Pins) of Welded Type 316L SS Inlerrupted after
_.p = 3.0%: (a) Base, and (b) Weld a nd('_ = I x lO -7 s-I).
a b 40 _rnI_-_.L----.I
Fig. 1 I. SEM Photomicrographs of Hole Regions of Incoloy
825 Interrupted after _p = 3.0%: (a) Exposed to
Liquid, and (b) Expo.t,:ed Alternately to Liquid and
Vapor (t =1 x 10 -7 s"l).
![Page 29: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/29.jpg)
21
o b
Fig. 12. SEM Photomicrex.jraphs oi" Hole Regions: (al
Incoloy 825, I mle with Pin, Interrupted after t'p =1.2%, (b) Incoloy 825, Hole without Pin, Inter-
rupted after £p = 1,2%, (c) Cu-30%NL Hole with
Pin, rp .-- 1.3%, and (d) Cu-30%Ni, Hole without
Pin, Interrupted after £p = 1.3% (£= I x i0 '7 s-l).
Rewriting Eq. 1 in the following form:
.. _ ITI
_-r_= _'e , ( 5 )
(where ep = e - s/E) and substituting Eq, 5 in Eq. 4 yields
Equation 6 can also be expressed as
_" I_ "!j.+. lI___.,1 ) (7)+
where _ = _,-,/Zp.Because K Isknown (forthe SSR'I,"specimen containing a through---holeK
= 3), Eq, 7 can be solved with the smooth-sp_Imen stre,.ss/straln data to estimate the
![Page 30: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/30.jpg)
22
actual stress concentration factor I_ at the hole. The actual strain concentration can thenbe determined by using Neuber's rule (Eq. 3).
Strvss/strain curves were determined for ali the materials from conventional tensiletests in air at a strain rate of-4.7 x 10-4 s-l. These stress/strain data were analyzed by theRamberg and Osgood equation and Neuber's rule to determine the strain concentration atthe hole as a function of plastic strain. As can be seen from Figs. 13 and 14, the results forCu and Type 316L SS show that the strain concentration factor decreases with plasticstrain, as expected.
Strain concentration Ke can also be computed by applying a simple power law relationbetween stress and plastic strain, namely,
E
1 Ewhere n = _ and C;o= _t-_• Locally, near the hole,
Kao = cro(K_tp) n' (9)
Equations 8 and 9 imply that
Ko--Kt (10)
Substituting Eq, I0 in Neuber's rule, Eq. 3,
K2 =K n+l, (II)
and solvingforK_,
Kr_= K2/(l+n) (12)
The two approachesforestimatingICegivealmostidenticalresultseven forrelativelylowplasticstrains,as illustratedirtFigs.13 and 14.
The localstrainsin Tables 11 and 12 arecomputed under the assumptionthatthestress/straindatageneratedat -4.7x 10-4s"Iat room temperaturecan be appliedtotheSSRT resultsat a much slowerstrainrateand at a slightlyhighertemperature.Thenominal strainin theunreduced sectionisdeterminedfrom the stress/stralncurve
correspondingto the loadat which the SSRTs were interrupted_The strainconcentrationfactorisdeterminedfrom Fxl.12 with a valueofn appropriateforthe strainin the tests.The localplasticstrainsrangedfrom 8.1to 15.2% forthetestsatthe strainrateof10-7 s-! {Table1I)and are lower{2.3-4.5%)fortestsconducted at the strainrateof] ft- S .q-I !Table 12).
!--
-!=W
![Page 31: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/31.jpg)
23
0
o6 _ e
_4
o Ramberg and Osgood Equation
._ 2 _-, Power Law between Stress and Plastic Strain
L-- • ,s, . _ I _,, _ .
! l
0 1 2 3 4 5Plastic Strain (%}
,P'O. 13. Strain Concentration Factor as a Function of PlasticStrain for Cu
F- , , i
08 '="._ F'-cc
= e
L
o4u L
0 i c_ '_Jn'bcr_'ar:dOs'°°dEquati°n J_
._ 2 - "_ Power Law between Stress and Plastic Strain '
F,.... I,--- , .... 1 , !:__
0 1 2 3 4 5Plastic Strain (%)
Fig. 14. Strain Concentration as a Function of Plastic Strainfor Type 316L SS.
iIi-I
|i
_i
![Page 32: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/32.jpg)
24
3.2.3 Relative SCC Susceptibility of Waste Container Materials
To obtain additional information on the relative cracking susceptibility of the variousmaterials, the load-deformation behavior of the specimen during the SSRT test wasanalyzed, and a cracking index parameter or stress ratio (SR) was formulated by comparingthe stress in the environment with that in air at the same plastic strain. For the present
geometry, the SR, which characterizes the effect of the environment on the capability ofmaterial to sustain load in the plastic range, can be defined as
1131SR = _aalr _ ay / 3)_p'
where Sen is the nominal stress in the environment, aair is the nominal stress in air
evaluated at the same plastic strain, and Cy is the yield stress of the material (see Table 9).To minimize geometry effects, Oen and _air are determined for the same specimen
geometry. Local plastic yielding is assumed to occur when the nominal stress reaches
ay/3, because the stress concentration factor for the present specimen geometry is =3.The use of stress instead of load eliminates any possible differences resulting fromvariations in specimen diameter. The SR focuses on the changes in stress after plastic
yielding, because SCC is not expected without plastic deformation. By eliminating theelastic contribution to stress, the SR appears to provide a sensitive indicator of SCC and isuseful for screening materials, at least qualitatively. As currently computed, we assumethat the differences in strain rate between the In-air and SSRT values do not significantlyaffect the stress/strain response at the temperature of interest. With no cracking, SR = I,and if the material is susceptible to cracking, the value is < I. However, a measured value of
1 may indicate only that the degree of cracking is so small that the change in loads cannotbe detected. Although values of SR < 1 indicate that cracking has occurred, tests atdifferent strain rates are needed to determine whether the cracking is environmentallyassisted.
To determine the SR, the strains in the SSRT must be known. By measuring the
pull-rod displacement during the test, we can determine the strains in "real time" byfinding the compliance of the SSRT machine and then using the measured compliance tocompute the strain from the measured loads and displacements, as is done in aconventional tensile test. Because the pull-rod displacement measurements were not
made for the first 13 tests, "post-test" estimates can instead be obtained from themeasured final plastic strain and load at the time of interruption of the tests. The totalstrain at the end of the test efinal is then
=ep(final) +a.._E' (14)£final
where the stress is computed from the final load and the initial cross section of thespecimen. The total strain of the specimen as a function of time, e(t), is computed byassuming a constant strain rate _.
e(t ) = efinal - t( t final ). ( ] 5 )
The plastic strain as a function of time, ep(t), is then
![Page 33: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/33.jpg)
25
_p(t) = E(t)_ a__Et " (16)
Calibration tests show that the assumption of a constant strain rate is quite good, once
yielding has occurred. Thus, plastic strains greater than -0.5% may be accuratelydetermined.
Figure 15 shows the variation of SR with plastic strain at a strain rate of 10--7 s-I forthe six materials in J-13 water at 93°C. The ranking of materials in order of increasingresistance to cracking is '1_'pe 304L SS < Type 316L SS < Incoloy 825 and Cu-30Ni < Cuand Cu-7Al. Thus, P-deoxid 'ized Cu and Al bronze appear to be more resistant to cracking
than the other alloys. The higher cracking resistance of Incoloy 825 relative to Type 304LSS can be attributed to the higher Ni content of Incoloy 825 and is qualitatively consistentwith SEM observations of the cracks. The differences in cracking behavior of Incoloy 825.
Cu-30Ni, Cu, and Cu-7Al are small, a finding that is also qualitatively consistent with theSEM observations. Also, the SR appears to be fairly sensitive to cracking even when the
cracks are too small to be readily observed metaUographically.
lt is clear that a greater change in stress/strain response in the environment than in
air is produced in the more SCC-susceptlble Type 304L SS than in the more resistantIncoloy 825 or copper and its alloys. A difference is also observed in the stress/strainbehavior of the smooth specimen and the specimen with two holes in air; this is
qualitatively consistent with the behavior expected from a reduction in cross-sectionalarea. For example, an 0.8-0.9 rnm through-hole in the gauge section causes a reduction inarea of-20%. But the difference between stress/strain response of the specimen withholes and that with holes and cracks cannot be explained on the basis of a reduction in
area because the enlargement of the holes due to observed cracking is small. Therefore itis possible that part of the shift in stress/straln curve of the specimen in the environmentrelative to that in air can be attributed to the difference in strain rates used for tests in air
and tests in tile environment, at least for Type 304L, which is known to exhibit anelastlc
effects at low temperature. °
A strain ratio analogou, to the SR can be defined:
.Ep(air)l , (17)£p(en) j_
where the strain in air and in the environment are evaluated at the same nominal stress.
A.,_can be seen from Fig. 16, the SCC susceptibility rankings determined from the twora_tG_ jre similar. However, the strain ratio Indicates a greater degree of susceptibility for
Type 304L SS, relative to Type 316L SS, than is suggested by the SR. Values of the strainratio at the evd of the tests are included In Tables 11 and 12.
iJ!
![Page 34: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/34.jpg)
26
1 _ _ _ _ " '_ "_ _'_-_ +_ +_ _ A _ Amm _m xcxoxo _ _ u u x°xoXo _ x x
0 0.8 _ _ D D _ " _ _r_ O c c o (3 D [] 0
_06 oo oo ooo ooCO °c °° _
°' 1m + Cu-7A1
acu_0.4 X Cu-30Ni /
O Incoloy 8250.2 [] 316L
O 304L, t i •
a I , _ I ' , J.--.--_ --
0 0.5 1 1.5 2 2.5 3 3.5 4Plastic Strain (%)
Fig. 15. Relative Cracking Susceptibility of Six CandidateMaterials in Simulated Well J- 13 Water at 93 °C.
Cracking susceptibility is expressed in terms ofthe nominal stress ratio [Eq. (13)] where lower
values imply greater cracking susceptibility(_ = I x 10 -7 s-I).
3.2.4 SCC Susceptibility of Weldment Specimens
The results of SSRTs on weldment specimens of several materials are summarized in
Table 12. The variation of SR with plastic strain or elongation for Types 304L SS and 316L
SS, Incoloy 825, Cu, and Cu-30Ni (Figs. 17-21) suggests that welding has a moredeleterious effect on the cracking of Cu and Cu-30Ni than on that of the austenitic alloys.Because the heats of the base materials used in the fabrication of the Incoloy 825, Cu, andCu-30Ni weldments were different from those used for the unwelded specimens, it is
necessary to clarify the role of heat-to-heat differences in these tests compared withdifferences associated with welding. The SEM observations of the base metal used in the
unwelded specimen (Fig. 1la) and the heat of the base metal used in the weldment (Fig.7a) show different cracking behavior, possibly associated with heat-to-heat variation. As is
shown in Fig. 22, the SR suggests that Incoloy 825 with the filler material Inconel 625 ismore resistant to cracking than is a similar weldment with the filler material Incoloy 65.
The composition of the latter is similar to that of Incoloy 825. Anomalous behavior hasbeen observed for Al bronze weldments produced by both GMAW and EBW. In these cases,
the observed SR ts greater than I (Fig. 23), and further work is necessary to explain this
unexpected behavior.
![Page 35: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/35.jpg)
27
o4 J : I . _,,, i I'
1.2 - x
Z_< _X _,X 6 x 6X XI - x x x x
_08 - <, o +o o4_
¢ 0.6 A Cu-7AI -I
.. x Cu o _" c = "J0.4 + Cu-30Nl D a
1
O Incoloy 825 u o a0.2 __316L []
O 304L o o o o o o0 i O O O O.... ' f , I _ .---L.. _ .,. '. = I
0,5 1 1,5 2 2.5 3 3.5 4Plastic Strain (%)
' /
/ ' Fig. 16. Relative Cracking Susceptibility of Six Candidate/ ,,
Materials in Simulated Well J-13 Water at 93°C.,,,
Cracking susceptibility is expressed in terms of
nominal strain ratio [Eq. (I 7)] where lower
values imply greater cracking susceptibility(t = I x 10 -7 s-I).
1.2 ' ' ' ' i
!I n
i
i_:.F10Q OO D DD r' C-'(2'= rhr_CC OD CDC o D D_
o 0.8 -Ji.iiiI_ o O O C 0 ,
0.6 o o o o c oo o o o o "1,.., i
_0.4o Base J
0 2 u Weld• I
1
I0 __.._._ I J I J , I i
0 0.8 1.6 2.4 3.2 4Plastic Strain (%)
Fig. 17. Comparison of SCC Susceptibility of Type. 304L
SS Base Metal and Weldment Speclmm_s inSimulated J-13 Water at 93°C ('E = I x 10 -7 s -I)
iiII
-m[]
![Page 36: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/36.jpg)
2t_
I 2 ...... ' '• ' I I ' i i " i i " i "" I i i
l
0 D D D 0 D D (3 [] [33
° Io08 oo oOO °o ° ]
°
_I 0 0 0 0 0 0 0 0
j_0.6
" t_0.4
0 Base t0.2 D Weld ]
]i I , t , L_ I , I , I , I _ I ,, I ,
0 0.8 1.6 2.4 3.2 4Plastic Strain (%)
r
F_g. 18. Comparison of SCC Susceptibility of Type 316LSS Base Metal and Weldment Specimens inSimulated J-13 Water at 93°C (e = I x _0-7 s-I)
.2 , 1 , i , i , .--i , , , , , l -
t,I F o°o ooooooOonoOoDO oOOo o o
0.80.6
_0.4 o Base
O Weld0.2
__L._ I L_ I , I , I , I ,,, I _ !-., L--... '--,l------
0 0.64 1.28 1.92 2.56 3.2Plastic Strain (%)
Fig, 19. Comparison of SCC Su.sceptibility of Incoloy 825Base Metal and Weldment Specimens inSimulated J-13 Water at 93°(7,('e= I x 10-7 s -I)
![Page 37: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/37.jpg)
29
.2 ' " _ I I I ' I I I ' I iI
f 'I 0 0 0 0 0 0 0 0 0 0 0 0 0 C C C m
13 Q D g D D O 0 D 0 D
_08 L-' ! r"J
_0.6 L ---,'
0.4 o [mse -
0.2 I OWeld jI-
0 F . ! , , ,, ! 2 , _ , J , , i
0 08 1.6 24 3.2 4
Plastic Strain (%)
F_g. 20. Comparison of SCC Susceptibility of Cu BaseMetal and Weldment Specimens in SimulatedJ-13 Water at 93°C (_ = I x 10-7 s"I)
1.2 --_, , , _ ' I _ "f , , !
2
1O 0 0 0 C 0 0 0 0 O = Q 0 0 C _
: n _ C O O O C C - - 3
o0.8
_0.6 I0 Base
_04
[]Weld ]: 0.2 -
i '0 --_--_L.---- _ _ J _ I , _ , f , ' , ! , I . ---]
0 07 1.4 2.1 28 35
Fig. 2,1. Comparison qf SCC Susceptibill_ of Cu-3ONiBase Metal and Weldment Specimens inSimulated J-13 Water at 93°C [e = I x 10 -7 s -I)
|1
![Page 38: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/38.jpg)
3O
O D D [] 0 D O O r- - C_"""u.uo °_u" - o o o o o o o o
0.72 ,i
c/l
0.48o Incoloy825/Incoloy65 _Veld)
0.24 o Incoloy825/Inconel 625 (Weld)
, l _ . ! I ! ' I , I , 1 -x---.- I , _ t _.u.--
0 0.64 1.28 1.92 2.56 3.2
Plastic Strain (%)
Pig. 22. Comparison of SCC Susceptibility of Incoloy 825Incoloy Weldment Specimens with twoDifjerent Filler Materials in Simulated J-13Water at 930(] (_ = I x 10 -7 s -I)
1.4 , , , j]1.2
0.8 J- t
0.6 o Cu-7Al (GM.AW) 7ra8 o Cu-7Al (EBM,9
0.4 1t_ Cu-TAI (['asc) i
O.2 ]l0 ,, L ._ : , _ _.._ ]
0 0.64 1.28 1.92 2.5_ 3.2
Plastic Strain (%)
Fig, 23. Comparison of SCC Susceptibility of Cu-TAl Base,Electron-Beam-Welded and Gas-Metal-Arc
Welded Specimens in Simulated J-13 Waterat 93°C (_ = I x 10 -7 s -I)
![Page 39: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/39.jpg)
31
3.2.5 Influence of Strain Rate on SCC
Figures 24-29 sh_:v the effect of strain rate on the SR for Types 304L and 316L SS,Incoloy 825, Cu, Cu-TAI, and Cu-30Ni at different plastic strains. The strain rate appearsto influence the SR of Types 304L SS and 316L SS, Incoloy 825, and Cu, but it has virtuallyno effect on the SR of Cu-30Ni and Cu-7AI. The effect is more pronounced for Type 304LSS than for Type 316L SS or the other materials. The lower values of the SR at a lower
strain rate suggest an increase in susceptibility to cracking typical of SCC. Similarly, theseresults suggest that the cracking observed for Cu-3ONi and Cu-7AI at the higher strain ratemay not be SCC. However, as pointed out earlier, both the exposure conditions and waterchemist y are different for the tests periormed at the two strain rates, lt appears that thestrain-_.,te effects on the SR are coupled with the environmental effects. More
specfficaily, the simulated J-13 water used for the slower strain-rate experiments in tests
on Types 304L and 316L SS and on Incoloy 825 are more oxidizing, which is reflected inthe higher values of specimen ECP (Figs. 24-26). A more oxidizing environment also tendsto lower the SR. As will be discussed later, even at the same strain rates, the change in the
SR appears to be correlated with the change in the specimen electrochemical potential(ECP). These results suggest that the ECP, pH, and other environmental variables must becontrolled to more clearly delineate the straln-rate effects on the SCC susceptibility ofdiffel ent materials.
3.2.6 Measurement of Crack Depth in SSRT Specimens
Attempts have been made to measure the crack depths by transverse sectioning ofthe SSRT specimens. In Type 304L SS (test W-4), multiple sections were examined by
alternately grinding away _4-5 mils of material and metallographicaUy preparing theresulting new surface. Even after as much as 20 mils of material had been removed in thismanner, only small cracks (_ 10 _m in depth) were observed. Even these cracks may beartifacts of the procedure used to produce the small-diameter holes in the gauge region.However, such cracks have not been observed in unstressed specimens with holes exposed
to simulated J-13 water at 93°C for the same length of time. Consequently, it appears that
we must modify our testing methods to produce cracks of greater depth. For exmnple, itmay be desirable to consider tests strained to failure under identical environmentalconditions so that the relative susceptibility of the materials can be quantified in terms ofmaximum crack depth and crack depth distribution or crack growth rate. This approach
may provide another means of resolving the relatively small differences in the crackingbehavior of the most resistant materials, and may also confirm some of the preliminary
findings of the interrupted tests. Further attempts to determine the crack depth inspecimens subjected to larger strains than in test W-4 will be discussed later.
3.2.7 influence of Water Chemistry on SCC
Tests W-1 and W-2 were performed on Incoloy 825 with different concentrations of
ionic species in the water, but at the same strain rate of 1 x 10-.7 s -I. The crackingbehavior in terms of SR (Fig. 30) appears to be very similar, The appearance of the cracks
in the two specimens as observed by SEM is also very similar. Although the water
chemistry is different for these two tests, the approximately identical stress ratio observed(see Table 11) is consistent with the ECP of the specimen (233--253 mV standard
hydrogen electrode [SHE]) measured in the two environments (Fig. 30).
![Page 40: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/40.jpg)
32
Tests W-5 and W-12 on Cu are similar, except that in test W-12 a small amount of
H202 was added to the feedwater. Although this addltlon did not significantly change theECP of the material, the lower SR (Fig, 31) suggests that H202 may be detrimental.However, it was difficult to observe differences in cracking by SEM.
3.3 SSRT Results (Tests W-23/W-33)
Because of the controlled water chemistry and water flow through the theenvironmental chamber as a result of introducing a mechanical pump discussed earlier,
several tests were repeated for the five candidate alloys, namely, Types 304L SS and 316LSS, Incoloy 825, Cu-30Ni, and Cu-7Al. As shown in Table 16, all but two of the tests wereperformed at a strain rate of 1 x 10 -7 s -I The tests for "l_ype304L and 316L SS involvedlarge plastic elongations, and these specimens were metallographically examined todetermine the deepest crack or crack distribution. Such observations would permit abetter understanding of the relative SCC susceptibility of these materials.
In addition, irl general, the tests (W-23/W-33) were generally Interrupted at higher
strains (ep = 5-18%) than were tests W-2/W-7 (ep = 3-4%) and these tests permitscreening of the five alloys under better-defined environmental and slightly lower ECPconditions than the early tests. Furthermore. for Type 304L SS, Incoloy 825. and Cu--30Ni, duplicate experimental results are obtained to check the reproducibility of
stress/strain data used to obtain SR, because the rankings of different materials used irl theprogram are solely based on stress or strain ratio, For Cu-30Ni and Cu-7Al alloys.experiments were performed at the slightly lower strain rate of 5 x 10-8 s-l to determine
any observable effect of strain rate on the SR. This strain-rate was chosen so that thesetests could be interrupted at higher plastic strains near those of tests run at faster strainrates within a reasonable length of time.
For previous tests (W-2/W-7). we have computed strains from the measured plasticstrain at the time of interruption and interpolated back by means of strain rate and time
(strain-rate method, Eq. i6). For tests W-23 and W-33, we have computed strains by
using both the strain-rate method and the displacement data from the dlal indicator onthe Jactuator. The extension data were recorded manually during the course ofexperiments, and these data, whlch are considered more accurate than those estimatedfrom the strain-rate method, provide a comparison of SR values obtained by the twodifferent methods. Additionally, for the last two tests (W-32 and W-33), an L_rDTextensometer was attached to the specimen, and the elongation strains estimated from the
displacement data provide another independent strain measurement. The data indicatethat evaluation of materials using stress and strain ratios is not affected by the manner inwhich the strains are computed in the SSRTs.
3.3.1 Crack Depth Distribution in SSRT Specimens
The SEM observations showed cracking in all specimens, and it was difficult to
quantify these observations to determine whether cracking is more severe in specimenssubjected to larger plastic strains and which material is most resistant to cracking.
![Page 41: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/41.jpg)
33
I _2 l _ i • "'i ,
o I _ .-I
" I¢Z0.8 co -t_t,,l'l c c o c ° ° O o o o o o o o
•.,0.6 -
"_ c: :Ec_r"D Swa.i.,_Rate.s "t= 0.4 _:._=_._ [ECP,mV(SHE)I
0.2 c lo7 131ol tr. 10"8 13431 J
0 0.5 1 1.5 2 2.5 3 3.5 4
Plastic Strain (%)
F_g. 24. Effect of Strain RaW and Specffnen FOP on SCCSusceptlbdiiIj of T_jpe 304L SS in SimulatedJ-13 Water at 93°C
.2 , , , , , ,
¢08 oooa ooO°oC
_0,6I¢1 -1
Strain RatP.. s¢,_ 0.4 [ECP. mV[SHE}I
0.2 o lo "7 {2r:,81-8c_ l0 [373]
0 0.8 1,6 2.4 3.2 4
Plastic Strain (%)
F_g, 25, Effect of StrataRate and S_ ECP on SCCS_scept_b_Itty of T_Ipe 316L SS in SimulatedJ-13 Water at 93°C
,,
![Page 42: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/42.jpg)
34
1 0 0 0 0 0 0 0 0 0 0 0 0 0
OOO_Domo __0
0.8
I_ 0.6
Strain Rate. s" I{/) 0.4 [ECP, mV(SHE)]
I o 10 .7 [253]
0.2 o 10 .8 [3181
i ! i I I _._.. | i I ' L__._L_.J _ [ . , l ___
0 0.64 1.28 1.92 2.56 3.2Plastic Strain (%)
Fig. 26. Effect of Strain Rate and Specimen ECP on SCCSusceptlbillhj of Incoloy 825 in Simulated J-J3Water at 93°C
1 • 2 -- -" i • l i -_ -''-''-'3-'-''--W'-'_'-'t'_W--'_ I .....
1 oO oo OOooooo oo oo o-
0.8 -= 0.6 -
-1
Strain Rate. sl/) 0.4 [ECP, mV(SHE)} !
o 10"7 13,33]
0.2 o lo.8 [2S_l
0 L-__J --- ' t.... 1 , i _.. t.._k__..___J_
0 0.8 1.6 2.4 3.2 4
Plastic Strain (%)
_., ,,)7 _.r¢,_,,i ni" ._Ir'nln Rntp. and SDedmen ECP o_I SCC__ A _19" _ • " ..,,jj....... v p ..........
_-i Susceptibility of Cu m Simulated J-13 Water ati 93oc.
"Ii
==ml_ , , .,
![Page 43: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/43.jpg)
35
"1.2 --" I _ I"' , ' ' _ ' /J
|
I - %9F_@a=°-- c o o o c o o
o 0.8 -= -I,4
0.6 1,_u--aJ.nRate. s" 1[ECP.mV(SHE)I
0.4 .7 qc lo [323] j
- 10.8 [2681 J0.2
,t_ , I _ I , I . __, ! L ! • I , '_ . I
0 0.64 1.28 1.92 2.56 3.2
Plastic Strain (%)
Fig. 28. Effect of Strain RaW and S,_clmen ECP on SOCSusceptibility of Cu-TAl in SbTlulated J-13 Waterat 93o(7,
1.2 .....,.... , , , , _---_ , _---F-
1 - 8od=o_rm_E.: .: c o o o o c o c c'"
008
0.6
Strain Rate. sI
0.4 [ECP, mV(SHE}]
0.2 C 10 .7 [not available]-8[] 10 1293l
0 0,7 1,4 2,1 2.8 3,5
Plastic Strain (%) "
Fig, 29. Effect of SO'am Rate and Specfmen ECP on SCC
.¢_,lce'prntthllit U ni" l'_JJ-3t')t_Tt tn Simulated J-13-_ Water at 93°Ci
:m
_j
|
![Page 44: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/44.jpg)
36
o08 -"
O. 6 Water Chemistry -Iii
[EOP, mV{SHEI]
ao.4o J13 (IX), [233l -J
4
0.2 u J 13(20x). 12531 t1
,L . _ _J 1 , , t , i _ I _: _ ..... I . , • ,_,i , ,..-!.l.,.--..,----J
0 1 2 3 4 5
Plastic Strain (%)
.Fig. 30. SCC Susceptibility of Incoloy 825, as Indicatedby the Stress Ratio for Tests with Different WaterChemistries under Approximately the Same ECPCondtlions at 93°C ('e = I x 10 ..7 s "i)
, 2 - " I " I '" I I " i ' '' 1 " = t _T _- 1 "' _"--
I 0 0 0 0 0 0 0 0 0 0 0 0 0 0 0 0
[] [] 0 C D _ 13 0 13 13 (3 [] 13
o0.8
_0.6 Water Chemistry
[ECP, mV(SHE)]
0.4 o without Hydrogen Peroxlde [303I
u with Hydrogen Peroxide [308]0.2
, 1 , .I...._.__,__ .... ! , . ! _<_..L__., t .... I _ ._.J.___,.__
0 0,8 I .6 2.4 3.2 z
Plastic Strain (%)
Fig. 31. SCC Susceptibility of Cu in Terms of the Stress Ratiofor Tests Conducted in Simulated Water withoutnnd lrlt'fh ~I.0 nnm H,_O,_ at 93fiC ('g = I x 10 -7 S -I)
:l
!I!
![Page 45: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/45.jpg)
37
Some preliminary results on Types 304L and 316L SS specimens suggest that it is
possible to detmmine crack depth distribution, even though the crack depths are smaller
than ,, 100 l_m. The crack depth distribution in a given specimen may be determined fromtransverse sections produced by alternately grinding off layers of _0.1--0.15 mm in
thickness, metallographically preparing and examining the resulting new section, and
determining the deepest crack observed, The distribution of crack depths observed on a
single transverse section in a Type 316L SS specimen (test W-24) is shown in Fig. 32. The
distribution of maximum depths observed in four to five transverse sectlons is shown for
both Types 316L and 304L SS specimens in Fig. 33. These results show that even in the
materials most susceptible to cracking in simulated J-13 water, the maximum cracking
observed is still small even after large plastic elongations. Therefore, the depth
distribution results for the materials may not be very useful in relating to the SR, at leastfor the materials and environment under consideration.
Table 16. SSRTs on Waste Container Materials at a Strain Rate 10 -7 s -I inSimulated J-13 Water at 93°C
i i,= J,,
Specimen
Te s t He at ECP Elongat ion, Kt aNumber Material Number (mV[SHE]) (%) (106 kg.m-l)
" ,, , ,,, ,, , ,, ___=r- ........ i
W-23 304L V70200 388 26.6 b 1.64
W-24 316L 16650 373 18.2 1.69
W-26 304L V70200 368 5.6 1.64
W'27 c Cu-30Ni 673 268 6. I 1.68
W-28 c Cu-7AI M 5485 258 5.0 1.43
W--29 Cu-7Al M5485 253 5.5 1.41
W-30 Incoloy 825 H2125F 328 5.7 1.75
W-31 Cu-30Ni 673 258 5.6 1.61
W-32 d Incoloy 825 H2125F 368 I 1.93 1.68
W-33 d Cu-30Ni 673 258 11.88 1.60
a Kt = machine and specimen stiffness; see Eq. 18.
b Test was run to failure; this is the failure strain estimated from the strainrate and time to failure.
c Tests were run at a strain rate of 5.0 x 10 -8 s -I
d For these tests, an LVDT extensometer was attached to the specimen topermit direct measurements of displacement in the specimen.
![Page 46: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/46.jpg)
38
0 i I I _ r _ t T , i ,
c
,_25 -o
¢;20 -
_15 L oo
_10 - o c o 4 _
,,_ c
5 - -0
l t I _ 1 i !, 1 ,
0 2 4 6 8 10
Location Number
Fig. 32. Crack Depth Distribution on a MetallographlcallyPolished Surface of a Transversely SectionedType 316L SS Specimen (Test W-24)
"_'50 , _ T , , .....
O D Type 316L SS (Test W-24), Ep = 18.2%¢_ 0 .Type304L SS (TestW-4), Ep=3.7%"40 -
_'_ O __30 - D c
_20 -
10 - o o0 0 0
0 0.1 0.2 0.3 0.4 0.5 0.6 0.7
Thickness of Material Removed (mm)
I_'_. 33. Maximum Crack Depth as a Function of MaterialRemoved for SSRT Specimens
I_m
=Ii
_I
![Page 47: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/47.jpg)
39
3.3.2 Relative SCC Susceptibility oi Waste Container Materials
For tests W-23/W-33, we have examined the effect of different strain computationmethods on calculated SR and reproducibility of the SR in duplicate tests performed onthree materials, namely, Type 304L SS, Incoloy 825, and Cu-30Ni. Once the most
accurate method of computing the SR and its reproducibility is established undercontrolled environments, it may then be possible to screen two materials for resistance toSCC even though the difference in the SCC susceptibility is qualitatively small.
For tests W-23/W-33, the stress or strain ratio can be computed by using threemeasurements: strains estimated from the strain-rate method, pull-rod displacementsfrom the dial indicator located on the Jactuator in the SSRT system, and displacements in
the SSRT specimen determined with the LVDT extensometer. For displacementsmeasured with the dial indicator, assuming that all of the plastic displacement ff_p) occurs
in the SSRT specimen, 5p is given by
where 8t Is the total displacement of the specimen and the loading system, P is the load,and Kt is the stiffness of the specimen and the machine. The dt must be corrected for anybacklash in the system. For the two SSRT systems, this backlash has been estimated 9 as0.0025 and 0.0038 cm, depending on the machine used. Kt can be calculated from 8t and
8p with the values at the time of test interruption. Here, 8t is obtained from the dialindicator and _ (Ep = 8p/L, where L is the gauge length of the SSRT specimen) is theplastic elongation determined by measuring the specimen length before and after the test.With the value of Kt thus determined, plastic strain can then be determined as a functionof nominal stress from the load-extension data for the tests under consideration. Thestress or strain ratio Is then estimated from the stress/straln data In a manner similar tothat discussed belbre.
For tests W-32 and W-33, the LvITr extensometer attached to the specimen was
used to obtain the displacement in the specimen as a function of P. For this case, _p is
given by
8p St-
where Ks is the specimen stiffness equal to 0.93EA/L, E is the Young's modulus, and A isthe cross-sectional area. The factor of 0.93 is introduced to account tbr the specimen
shoulder deformation. 1o The specimen stiffness values thus determined for Incoloy 825[test W-32) and Cu-30Nt [test W-33) are 1.56 x 107 and 1.23 x 107 kg.m" 1, respectively.
The plastic strain is computed by dividing the plastic displacement by L. From the plasticstrain determined as a function of nominal stress, the SR or the strain ratio is computed asbefore.
Figures 34 and 35 show the plots of stress and plastic strain for the three methods ofstrain computation for Incoloy 825 and Cu-30Ni, and the corresponding plots of stress
ii
![Page 48: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/48.jpg)
4O
'4
ratio versus plastic strain are shown in Figs. 36 and 37, respectlvely. As can be seen, themethod of strain computation has virtually no effect for Incoloy 825 and only a small effectfor Cu-30Ni at strains <6-7%. For both materials, the strain computation method using
the dial indicator and extensometer gives very good agreement. We will later examine theranking of different alloys in terms of increasing resistance to SCC on the basis of thesedata.
With regard to the reproducibility of the stress/strain response and SR fromduplicate tests on 'I_rpe 304L SS, Incoloy 825, and Cu--3ONi (regardless of the strains atwhich the test was interrupted), the results are in close agreement. Figures 38 and 39demonstrate that both the stress/strain plots and the corresponding plots of stress ratio
versus plastic strain for Type 304L are reproducible wlth no discernible scatter. Similaragreement has been obtained from duplicate tests performed on Incoloy 825 and Cu-30Ni,as shown in Figs. 40-43.
The SSRT results from tests W-2/W-7 performed on different materials at a strain
rate of 10 -7 S-I are compared with results obtained from tests W-23/W-33, which wereconducted at the same strain rate but under slightly higher ECP conditions. Figures 44--48
display such comparison plots of stress ratio versus Ep for Types 304L, 316L SS, Incoloy825, Cu-3ONi, and Cu-7AI, respectively. Because the extension measurements by dialindicator are not available for tests W-2/W-7, we used the strain-rate method to compute
the results. Figures 44-48 show that the disagreement between the two tests is slgnificantfor Type 304L SS (W-4 and W-26, Fig. 44), "l_pe 316L SS (W-6 and W-24, Fig. 45), Incoloy825 (W-2 and W-32, Fig. 46), and Cu-30Ni (W-3 and W--33, Fig. 47). However, [.here isclose agreement between the results of two tests (W-7 and W-29, Fig. 481 for Cu-7Al,which also happens to be the most crack-resistant material. Similar comparison data forCu are not avallable.
The disagreement in results for the four alloys cannot be reconciled in terms of the
method of computing strains (because all the methods discussed in thls report essentiallylead to approximately identical results), but instead appears to be associated with the
change in environmental and exposure condltions. In fact, the disagreement in results isbetter correlated with specimen ECP, at least for Type 304L (Fig. 441, Type 316L SS (Flg.45), and Incoloy 825 (Fig. 46). In particular, the higher specimen ECP tends to give a
lower SR, i.e., higher specimen ECP consistently results in g_Jater susceptibility. Fortests conducted under approximately the same ECP conditions, almost identical results for
the SR are obtalned, as shown in Figs. 30, 39, 41, and 43. lt is important to note thatdespite the vast difference in water chemistry for tests W-1 and W-2 (Fig. 301,
approximately identical values for the SR are obtained. This is consistent with the fact thatthe same ECP values were measured in these two tests. Although it is easy to comprehend
why a slightly more oxidizing environment produces a greater susceptibility to cr,_ckingwith a resultant decrease in the SR, it is more difficult to obtain a fundamental
understanding of how a shift in ECP value in the range of 250--380 mV(SHEI can affect thecracking susceptibility of austenitic stainless steels in simulated J-13 water at 93°C. Sucha shift in ECP has not been found to significantly affect the SCC susceptibility of .Types 304and 316L SS under boiling-water-reactor operating conditions.
![Page 49: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/49.jpg)
4 1
550 _. , , . _ .... ,..-_----r--,---.
500
450m 400
l.i"_ 350
30 0 o Dial Indicatora Interpolation by using strain and strain rate
250 ' ' ' ' ' "' ' " ' ' ' ' '"0 2 4 6 8 10 12 14
Plastic Strain (%)
Flg. 34. Nominal Stress Versus Plastic Strain for Incoloy
825 (Test W-32) Specimen in Simulated J-13Water at 93°(?, (e = I x 10 -7 s -l)
300 , , • , . , ... , ,
250
"_' 2000.
150
100 .-I" o Extensometer
5 0 L_ _ Dial Indicator[ a Interpolation by using strain and strain rate
0 L_ _ ' • i _ I , I _,.----J----,-. I ,
0 2 4 6 8 10 12 14
Plastic Strain (%)
Fig. 35. Nominal Stress versus Plastic Strain for Cu-3ONi(Test W-33_ in Simulated ,.I-13 Water at 93°C
(t : I x lo-z)
i-|
![Page 50: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/50.jpg)
42
1.2 , _, ]
o08 -olul
0.6
0.4 o ExtensometerD Dial Indicator
0.2 _ Interpolation by using strain and strain rate _
0 2 4 6 8Plastic Strain (%)
Fig. 36. Variation of Stress Ratio with Plastic Strain forIncoloy 825 (Test W-32) in Simulated J-13Water at 93°C _ = I x 10 -7 s -l)
.2 ..... , , -. i
o 0.8 _ -
0.6
_0.4o ExtensometerD Dial Indicator
0,2 a Interploation by using strain and strain rate
, , I .... J I • ---
0 2 4 6 8Plastic Strain (%)
F_g.37. Variation of Stress Ratio with Plastic Strain forCu-3ONt (Test W-33) in Simulated J-13 Waterat 93°C _ = I x 10- 7 s "I)
![Page 51: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/51.jpg)
43
600 ---,---,- _. , , ... .....r---,--_ . , - _---
48O
'360 _)_).,_o _(=_o
24o_ -7 -I
Strain Rate, I0 s
120o Test W-23n Test W-26
• I ,_.._. I I I i I , l , .... I ,
0 4 8 12 16 20 24 28 ,,
Plastic Strain (%)
Fly. 38. Nominal Stress versus Plastic Strain for Type304L SS in Simulated J-13 Water at 93°C.
A dlal indicator was used to estimate strains
in the SSEI" specimen.
1.2
1Strain Rate. 10 -7 -1
= 0.8oll
eJ
_0.6 - _ _ _ o_
0.4 TestNumber[ECP, mV(SHE)]
o w-23 13881 _j0.2 - !
m W-26 [368]]
____ _ _ , I , _ , ,
O 2 4 6 8
Plastic Strain (%)
F_g. 39. Variation of Stress Ratio versus Plastic Strain for
Type 304L SS in Simulated J-13 Water at 93°C.A dlal indicator was used to estimate strains
in the SSRT specimen.
![Page 52: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/52.jpg)
44
600 , , , , , , , ,------
480 D_ -
_" 360 _
240 -7-1 -Strain Rate, 10 s
1 2 0 o Test W-30[3 Test W-32
0 2 4 6 8 10 12 14
Plastic Strain (%)
Fig. 40. Nominal Stress versus Plastic Strain for Incoloy825 in Simulated J-13 Water at 93°C. A dial
indicator was used to estimate strains in the
SSRT specimen.
Io2 ......... ,
o 0.8IM
c_I_ Strain Rate, 10"7s "I
0.6 -
Test Numberv_ 0.4 [ECP, mV(SHE)I 1
o W-30 I3281
0.2 a W-32 [368]
0 , , I , t , 1, , "]"
0 2 4 6 8
Plastic Strain (%)
Fig. 41. Variation of Stress Ratio versus Plastic Strain forIncoloy 825 in Simulated J-13 Water at 93°C. Adlal indicator was used to estimate strains in the
SSRT specimen.
![Page 53: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/53.jpg)
45
400 , • -T----' , ' , ' ,""--'-'-'r---'-'--'-
300
'_' DE] DO DDE_3
200 _ _'_ _
rqD
oO
C/) Strain Rate, I0 "7s" 1
I00o Test W-31
o Test W-33
0 _ L , I _ ,l, A I _ I _ I , .
0 2 4. 6 8 10 12 14
Plastic Strain (o,_)
Fig. 42. Nominal stress versus Plastic Strain for Cu-TAlin Simulated J-13 Water at 93°C. A dlalindicator was used to estimate strains in the
SSRT specimen.
.2 , .... , , ....---.,, , -----.----_
1
..00.8+.1
m 0.6 Strain Rate, 10
0.4 Test Number: [ECP, mV(SHE)I
0,2 o W-31I258]n W-33 [258]
, _ I , ,,, I .... _ I __ b .....
0 2 4 6 8
Plastic Strain (%)
Flg. 43. Variation of Stress Ratio versus Plastic Strain for: Cu-3ONi in Simulated J-13 Water at 93°C. A
dial indicator was used to estimate strains in the
SSRT specimen.
![Page 54: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/54.jpg)
46
I ,2 -' ' I '"--_ ' '
o 0.8
oooOOOCOooo°°° o_Do-"= 0.6
_oooo_"ocDooooooooo
_ 0,4 Test Number
[ECP, mV(SHEll
0,2 o W-4 [3101n W-26 [368]
0 -- ,, , I , I _,, ' * -
0 2 4 6 8
Elastic Strain (%)
Fig. 44. Comparison of Stress Versus Plastic Strain forTwo Tests on Type 304L SS in Simulated J-13Water at 93°C (_ = I x 10 -7 s -I)
.2 ,, ,, , , , , .......
O 0.8 oooooOOO°°O° o o
cOoO o o o o o o []= 0.6 o °°_- o
Test Number(/_ 0,4 o [ECP, mV(SHE) 7
1
o W-6 [268]0.2 o W-24 [373]
0 , I ._-....--_.__ I , ' .
0 2 4 6 8
Plastic Strain (%)
I_. 45. __omparison of Stress Versus Plastic Strain forTWo Tests on Type 3161., SS in Simulated J-13Water at _3 °C (_ = 1 x 10 -7 s " I )
![Page 55: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/55.jpg)
47
1000000000C3000
o0.8
mO.6Test NumberIECP. mViSHE)]
_0.4o w-2 [2531o w-32 [368l
0.2
0 2 4 6 8Plastic Strain (%)
FIg. 46. Compcu'L_on of Stress Versus Plastic Strain forTWo Tests on Incoloy 825 in Simulated J-13Water at 93'(7, _ = I x 10 -7 s-z)
,2 a ] I I , I 1
• +
1 -O00000O OC S SZ)0
o O.8 ___r'_'-" ":_'-'_
® 0.6
Test Number
0.4 _.. [ECP, mV(SHE)]
0 W-3 [not available]
0.2 i- = W-331258]i ,. ! ........ -- ; .... .
0 2 4 6 8Pla.st.i¢ Strain (%}
Pig. 47. ComparLson of Stress Versus Plastic Strain for_ ,T,...._..^.. ¢'_,,_¢_¢_J_ _ C:_m,,Iw.,t._,-I..,.r_ _ "4 llJ't_'_"
at 93_C _ = I x10 -7' s"l}
![Page 56: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/56.jpg)
48
o 0.8
_ 0.6
Test Number
¢J_ 0,4 [ECP, mV(SHE)]
0 W-7 [323]0.2 o W-29 [253]
_ , _.,,___..._ I .__..__, I ...... ,
0 2 4 6 8
Plastic 8train (%)
Fig. 48. Comparison of Stress Versus Plastic Strain forTwo Tests on Cu-7Al in Simulated J-13 Waterat 93°C _ = I x10 -Ts -I)
We can examine the ranking of the five alloys in terms of stress and strain ratiosestimated from the dial-indicator and extensometer measurements of displacements in
the specimen from tests W-23/W-33. Figure 49 is a plot of stress ratio versus plasticstrain for the five candidate materials based upon the dial indicator readings. In this plot,
we have included the duplicate test results for Type 304L SS, Incoloy 825, and Cu-30Ni
(represented by the same symbol for each mater]al). On the basis of this plot, the rankingof materials in order of increasing resistance to cracking is Type 304L SS < Type 316L SS
< Incoloy 825 < Cu-30Ni < Cu-7AI. These results are similar to the ranking for tests W-2/W-7 except that Incoloy 825 appears to be slightly inferior to Cu-30Ni in crackingresistance. A similar ranking is observed when the strain ratio is used (Fig. 50). The
slightly superior SCC resistance of Cu-30Ni compared to that of Incoloy 825 can also beseen from Tests W-32 and W-33, where specimen displacement measurements were
made with the LVDT extensometer. Both of the tests for this case were interrupted at
-12.0% elongation, strains. The slightly superior SCC resistance of Cu-30Ni, compared to
that of Incoloy, in terms of both stress and strain ratios is shown in Fig. 51. lt is importantto note that the above ranking for the five materials is again not affected by the method of
computing strain, as is evidenced from Figs. 52 and 53, where stress and strain ratios areestimated from the measured plastic strain and strain rate. "[_e significance of the slightdifferences in resistance to SCC observed in this study for the two competing materials
(Incoloy 825 and Cu-30 Ni) requires a better understanding of the stress and strain ratios,-" as weU as conltrmatlon by omer types of tests such as ira_;wrv-m_-c,am_ _._ _c_L=.
i
-B
B
,m
![Page 57: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/57.jpg)
49
,2 _. ' • J • ' ..... r_' • .... i
1 4 A 4& A& •
o 0.8'_ ee ooe o® =e_ o4o
_ 0.6 o_ _ a_o o©
0.4 • Cu-7A]o Cu-30Nt
,, Incolo:, 8250.2 , 316L
0 304L
..... _ ] ..... , .... I _ ___ I .......
0 2 4 6 8Plastic Strain (%)
Fig, 49, Relative. Cracking Susceptibility of llve Alloys irtSimulated J-13 Water at 93_C, Cracking suscepti-
bility is expressed in terms of the nominal stressratio [Eq, (13)] where lower values imply greatercracking susceptibility. Stress ratio is based onestimating strains n the SSRT specimens bN meansof a dlal indicator (_ = I x 10 -7 s-l).
Cu-7AI
o Cu-3ON! • A •
1 ,, Incoloy825 4 4 A A•e 316L
0 0.8 o 304L %,_ %_. =o oD
o o ata a a_ aaaa ell em
_0.6 _ •A •
0°4 , °
0.2
o ,0 2 4 6 8
Plastic Strain [%)
Fig. 50. Relative Cracking Susceptibility of Five Alloys inSimulated J-13 Water at 93°C. Cracking suscepti-
bility is expressed in terms of the nominal strainratio [Eq. (I 7)] where lower values imply greatercracking susceptibility, Strain ratio is based on
estimating strains tn the _: specu'nens by meansi of a dial indicator (_ = I x I0 -7 s).
=iJ
=
ql' lt '' " _tl_l' trl_
![Page 58: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/58.jpg)
5O
I •2 _--_ .........I I ' • ' ' _'I " _"
o I
0.8 - ._"-""_"_"- "
0.6
w 0.4 _ Stress Ratio Strain RatioW
°0.2 • Cu-30NI ,, Cu-30Ni _O Incoloy 825 o Incoloy 82[
0 , I , ....... I , -L,.- J .....
0 2 4 6 8Plastic Strain (%)
Fig. 51. Cracking Susceptlbflity of Incoloy. 825 and Cu-3ON_in Terms qf the Stress Ratio [Eq. (13)] or the StrainRatio [Eq. (I 7)] In J-13 Water at 93°C Where Lower
Values Imply Greater Susceptibility. The stress andstrain ratios are based on estimation of strains in the
SSRT specimens by means of an LVDT extensometer.
_ 0.8 , • " *'* "" *@ • @ @ ._,_r_O000000000,6 @ ,._u_,.,-
ooOOOO OOOO'_" A Cu-7AI
a Cu-30Ni0.4 _ Incoloy 825• 316L
0.2 o 304L
0 2 4 6 8Plastic Strain (%]
Fig. 52, Relative Cracking Susceptibility of Five Alloys InSimulated J-13 Water at 93°C. Cracking susceptl-
bflity is expressed in terms of the nominal stress ratio
[Eq, (13)] where lower values imply greater crackingsusceptibility. Stress ratio is based on estimating
_ rate method [Eqs, (15) and (16)].___
_,|
.!I
![Page 59: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/59.jpg)
51
'I.2 %, r ......... _ . , ....._AAA_
I A Cu-7AI aaa AA a_,a_,A,,_tD Cu-30N!
0.8 a Incoloy 825
316! _n,_""o°cr'OD°°°°°°• _e L%A_O 304L .[Dnu .A_aa_
1 0.6 #_A%tX" . " " " "0.4 _ • •a @
012 *
• ..oOO0000
0 ......,." ___ooooooOC,_" . j.........0 2 4 6 8
Plastic St.m_
Fig. 53. Relative Cracking Susceptibility of Five Alloys inSimulated J-13 Water at 93°C. Cracking suscept_-billty is expressed in terms of the nominal strainratio [Eq. (I,3)] where lower tw,_lues imply greatercracking susceptibility. Stress ratio is based on
estimating strains in the SSRT specimens by meansof the straln-rate method [Eqs. (15) and (16)I.
3.3.3 Influence of Strain Rate on SCC
Two tests (W-27 and W-28; see Table 15) have been performed at the slower strainrate of 5.0 x 10--8 s-I, one on Cu-30Ni and another on Cu-TAl. Comparison of the results
wlth those obtained at the slightly higher strain rate of 10-7 s-I showed no significanteffects of strain rate on stress ratio. However, these tests show the potential for studyingthe effects of strain rate on cracking with the use of stress or strain ratios and hence forestablishing whether the cracking ts environmentally assisted.
3.4 Preparation and Analyses of Test Solutions
The effluenbwater chemistries for the completed SSR:I" tests are reported in Tables
17-20. In test W-1, the concentrations of most of the species were higher by a factor of=20 relative to J-13 water; however, the values for Ca and Mg were very low (<0.04 ppm)to prevent precipitation of slightly soluble compounds such as CaC03, CaF2, MgF:_, CaSIO3,and MgSiO3. The HCO_ concentration was obtained by bubbling a 12% C02-20% 02--68%N2 gas mixture through the feedwater and maintaining a 5 psig overpressure in thefeedwater tank. This gas mixture, also set the dissolved-oxygen concentration of the
-- feedwater at ,,7-8 ppm. The I4CO_ concentration in the effluent water was higher by ao factor of only .,6 than that in J-13 water because some of the CO2 escapes into the
j atmosphere in the test vessel at 93°C. The relatively high concentration of sodium silicate
-i and low concentration of HCO_ are reflected in the rather high pH value of =9.2.
Precipitation of silica compounds on the Incoloy 825 SSRT specimen and the test vessel==' also occurred with this nominal 20x water chemistry.
-!11
!
![Page 60: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/60.jpg)
52
Table 17. Chemical Composition a of Effluent Water from SSRTs on Candidate WasteContainer Materials, Tests W-I through W-9
Component or Test NI4mbers .............Parameter W- 1 W-2 W-3 W-4 W-5 W-6 W-7 W-8 b W-9 b
Composition
[rag/L)Ca 0.04 18.4 15,5 14.5 5.2 7.3 7. I 5.16 3.07
Mg <0.01 1.94 1.89 1.92 1.75 1.83 1.81 1.81 1.75Na 937,0 49.7 48.3 47.9 47.8 49,3 49.4 48.4 50.1
K 106.0 5_53 5.56 5.52 5.72 5.61 5.63 5.23 5.37
Li 2.44 0.13 O. 13 O. 13 0.06 0.09 0.09 0.06 0.06
Fe 0,75 <0.01 <0.01 0.01 0.01 <0.01 <0,01 0,01 <0.01
Mn 0.02 0.01 0.01 0.01 0.03 0.02 0.01 <0.01 0.01
Al O. 55 <0.1 <0. I <0. I <0.1 <0.1 <0.1 <0, 1 <0,1
Si 530,0 30.2 29.4 29.6 27.6 29,1 29.2 0.42 0.18
F- 43.0 2,2 24,0 24.0 31.0 25.0 26.0 2.6 2.2
Cl- 117.0 12.0 12.0 12.0 7.6 I0.0 9.8 6, 1 6.6
NO_ 194,0 20.0 20.0 20.0 12.0 16.0 16.0 9.2 I0.0SO_- 350.0 19.0 19.0 19.0 17.0 18.0 19.0 18.0 20.0
HCO_ 622.0 78.0 44.0 36,0 15.0 25,0 19.0 55.0 52.0
CO23- c c c c c c c 9.0 13,0
TDS d 2902.7 237.0 219.8 210.5 170,8 187.2 183.0 161.0 164.4
pH25oc 9.21 7.82 7,35 7.33 7,32 6,86 6,89 8.88 9,11
Conductivity
[gS/cm) 4400 425 425 425 375 375 375 325 325
a Cation and anion concentrations determined by ICP spectroscopy and ion chroma-tography analyses, respectively, with the exception of HCO_. which was obtainedby titration.
b Approximately I ppm H202 was added to the feedwater.
c Not analyzed.
d Total dissolved solids.
4....... IVr'"II '' '"'''ill,'_I''FI',I_,_ ' 'P Imqlllr' ''liD'=" "I111'..... I_ al, ='Ilrl,qllilP,_,IIPllf", IU,,ii,,, .... lr I111qil,_I_ _Ii ri_'ie_i_
![Page 61: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/61.jpg)
53
Table 18. Chemical Composition a of Effluent Water from SSNFs on Candidate WasteContainer Materials, Tests W-lO through W-18
Component or Test NumbersParameter W-10 W-ll W-12 W-13 W-14 W-15 W-16 W-17 W-18
Composition{rag/L)Ca 10.2 11.0 10.5 10.9 10.6 10.6 10.8 10.8 10.5
Mg 1.79 1.84 1.78 2.08 2.04 2.19 2.07 2.06 2.08Na 51.6 49.6 47.4 55.6 51.6 52.7 52.0 51.8 49.6K 5.23 5.33 5, 11 6.09 5.43 5.96 5.86 5.41 5.88Li 0.06 0.06 0.05 0,07 0.06 0.07 0,06 0.06 0.06
Fe <0.01 <0.01 <0.01 <0.01 <0.01 <0.01 <0.01 <0.01 <0.01Mn <0.01 <0.01 <0.01 <0.01 <0.01 <0. I <0. I <0. I <0.1AI <0.1 <0. I <0.1 <0.1 <0.1 <0. I <0.1 <0. I <0. ISi 0.13 <0. I <0.1 b b b b b bNic 0.46 1.66 ! .23 1.06 0.85 0,94 1.41 1.78 1.65
F- 2.0 1.9 1.8 2.2 2.1 2.0 2.1 2.1 2.1Cl- 6.5 6.4 5.8 6.9 5.9 6.4 6.2 5.9 6.6
NO-._ I0.0 10.0 9.9 11.0 I0.0 10.0 I0.0 I0.0 10.0
SO4_- 19.0 18.0 17.0 21.0 20.0 20.0 19.0 20.0 20.0HCO_ 128.0 133_0 128.0 137.0 125.0 130.0 133.0 133.0 131.0CO2- d d d <6.0 <6.0 <6.0 d d <6.0
TDS e 234.9 238.8 228.6 254.0 233.6 241.0 242.5 242.8 239.5
pH25oc 8.51 7.98 7.76 8.33 8.34 8.31 8.26 8, I0 8.39
Conductivity(_S/cm) 375 370 350 365 370 395 385 405 400
a Cation and anion concentrations determined by ICP spectroscopy and ion chroma-tography analyses, respectively, with the exception of HC03-, which was obtainedby titration.
b Not analyzed; Si no longer added to the feedwater.
c Nickel is present from corrosion of the nickel test vessel.
d Not detected.
e Total dissolved solids.
![Page 62: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/62.jpg)
54
Table 19. Chemical Composition a oj'E._quent Water from SSRTs on Candidate Waste
Container Materials, Tests W- 19 through W-27
Component or Test NumhgrsParameter W-19 W-20 W-21 W-22 W-23 W-24 W-25 W-26 W-27
Composition
(rag/L)Ca 11.0 10.5 10,6 10,7 I0,5 10,5 10.8 10,8 10.8
Mg 2.13 2,15 2.32 2.31 2.17 1.91 2.22 1.88 1.99Na 50.3 50.1 50.9 51.0 50.5 50.7 51.5 50.9 50.9K 5,71 5,45 5.32 5.49 5.58 5,36 5.48 5,38 5,39
Li 0.05 0,05 0.06 0.06 0,06 0.06 0.06 0.06 0.06
Fe <0.01 ¢:0.01 <0.01 <0.01 <0.01 <0,01 <0.01 <0.01 <0.01
Mn <0,01 <0,01 <0.01 <0,01 <0.01 <0.01 <0.O1 <0.01 <0,01
Al <0. I <0.1 <0.1 <0, I <0.1 <0.1 <0. I <0. I <0.1
Si b b b b b b b b b
Ni c 1.54 0.83 1.22 2.23 I, 13 1.48 1.69 1.13 2.13
F- 2.1 2.2 2.0 2.0 2,1 2.0 2.2 2.2 2.1
Cl- 6,6 7.1 7,0 6.4 6.2 6.5 6.5 6.4 6.6
NO_ 11.0 11.0 12.0 I0,0 I0,0 11.0 12.0 12.0 13.0
SO4_ 20,0 20.0 2,',_O 20.0 19.0 18.0 20.0 18.0 19.0
HCO_ 134.0 134.0 133.0 130.0 133.0 137.0 141.0 139.0 142.0
CO23- <6.0 - <6.0 <6.0 d <6.0 d d d
TDS e 244.4 243.3 246.4 240.0 241.1 244.5 253.5 247.8 236.0
pH25oc 8,36 8.24 8.35 8.31 8.26 8.35 8.18 8.28 8.23
Conductivity
BS/cm 405 4 I0 400 395 385 395 375 375 380
a Cation and anion concentrations determined by ICP spectroscopy and ion chroma-
tography analyses, respectively, with the exceptlon of HCO_, which was obtained bytitration.
b Not analyzed; Si no longer added to the feedwater.
c Nickel is present from corrosion of the nickel test vessel.
d Not detected.
e Total dissolved solids.
!!
![Page 63: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/63.jpg)
55
Table 20, Chemical Composition a of Ej_fluent Water from SSR'rs on Candidate Waste
Container Materials, Tests W-28 through W-33
Component or , Test Number_Parmneter W-28 W-29 W-30 W-31 W-32 W-33
Composition
(rag/L)Ca 10.8 11.0 10,4 10.6 10.3 10.4
Mg 1.85 1.86 1.83 1.78 1.79 1.76Na 50.5 50.4 51.0 50.3 49.5 50.0
K 5.46 5.86 7.77 5.45 5.32 5.32
Li 0.06 0.06 0,06 0.06 0.06 0.06
Fe <0.01 <0,01 <0.01 <0.01 <0.01 <0.01
Mn <0 01 <0.01 <0.01 <0.01 <0.01 <0.01
Al <0. I <0. I <0. I <0. I <0.1 <0.1
Si b b b b b b
Nic 1.77 2.22 2.47 1.24 1.93 1.97
F- 2.2 2.3 2.0 2.1 2.2 2.1
CI- 6.4 7.1 9.4 7.1 7.1 7.1
NO3- 12.0 12.0 12.8 12.6 12.6 12.9
SO 2- 18.0 18.0 19.9 19.5 19.7 20.0HCO3- 14 I. 0 140.0 138.0 135.0 134.0 134.0
CO32- d d d d d d
TDS e 262.0 250.9 255.7 245.8 244.5 245.7
PH25oc 8.12 8.11 8.22 8.11 8.01 7.97
Conductivity(l_S/cm) 385 395 395 375 370 380
a Cation and anion concentrations determined by ICP spectroscopy and ion chroma-tography analyses, respectively, with the exception of I-ICOn, which was obtainedby titration.
b Not analyzed; Si no longer added to the feedwater.
c Nickel is present from corrosion of the nickel test vessel.
d Not detected.
e Total dissolved solids.
![Page 64: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/64.jpg)
In tests W-2/W-7, the efffluent-water chemistry more closely approximated that of J-
13 water; however, the concentrations of some of the anions (F-,CI-, and NO_), we_higher by factors of --2-20 and the concentrations of HCO_ were lower by factors of -2-4.
The 30-ppm Si (_80 ppm (--80ppm SiO 2-) and 78-19-ppm HCO_ in the feedwater wereobtained by adding Na2Si03 and bubbling with a 12% CO2-20% 02-68% N2 gas mixture, asin test W-1. The PH25oc of the effluent water ranged from 6.9 to 7.8 in these tests.Nickel from corrosion of the test vessels was also detected in the effluent water (typically
<2 ppm). To increase the HCO_ concentration to the level in J-13 water (i.e, to --143ppm), this species was added as NaHC03 and the gas mixture in the feedwater tank waschanged to 20% 02-80% N2 in Tests W-8 and W-9. Approximately I ppm of H202 was
also added to the feedwater after sparging with the 02-N2 gas mixture. The measured
H202 concentration in the effluent water was _0.2 ppm.
Beginning with test W-10, Na2Si03 was no longer added to the feedwater. "I_ereason for this change was that although silica solubility increases as temperatureincreases, the amount of material in solution depends on the phase (crystalline or
amorphous) in equilibrium with the water, as well as on the nature and concentration ofother species that are present.t1 The soluble form of silica is the monomeric speciesSi(OH)4, i.e., orthosillcic acid. Polysiliclc acid with molecular weights, as SiO2, up to100,000 ainu and particle sizes <50 }k in diameter, as well as colloidal silica with a range of
pm_icle sizes, can also be present in the water.
The "solubility" values range from --100 to 150 ppm as SiO2 at 25°C; at --100°C, therange is --400 to 500 ppm. At 25°C, minimal solubility of amorphous silica (=100 ppm)occurs at pH = 7; at higher and lower pH values, the solubility increases. But impurities inthe water can have a significant effect on the solubility of silica. For example, A1203 or
AICI3.(6H20) can adsorb on silica and cause it to precipitate (i.e., decrease the SiO2concentrations to <6 ppm}. This readily soluble hydrated salt was used to add Al3+ tosimulated J-13 water in our experiments. Also, magnesium ion converts soluble silica
(amorphous) to a magnesium silicate and also decreases the solubility. Organic impurities,although very low in our deionized water, can either increase or decrease silica solubility.Because silicates are commonly used as corrosion inhibitors in low-temperature
systems, 12,13 it is unlikely that they would contribute to SCC of the candidate materials inour tests.
Although the effluent water chemistries [n Tests W--8 and W-9 more closelyapproximate J-13 water (with the exception of Si), the HCO_ concentration was stillsomewhat lower (=50 versus 143 ppm} and the pH25oc was considerably higher (8.9 to 9.1versus 6.9). Because of the high pH, CaC03 precipitation occurred, as evidenced by the
high Ca content of the scale deposit and the low Ca values in the efflue_it water of Tests W-8 and W-9 (Table 17) relative to the feedwater (3-5 versus I I ppm).
In Tests W-10/W--23, the ionic species were of the same formulation as that in the
two previous tests, but a 12% CO2-20°/o 02-68% N2 cover gas was bubbled through thefeedwater to achieve the desired dissolved oxygen concentration and to produce an
"equilibrium" CO2 overpressure to stabilize the HCO_ concentration and pH of thefeedwater. As is evident in Tables 17-20, the HCO_ and pH25oc values in the effluent water
range from 125 to 141 ppm and 7.8 to 8.5, respectively. The effluent Ca and Mgconcentrations were virtually the same as in the feedwater, and very little deposition
![Page 65: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/65.jpg)
57
occurred on the SSRT specimens or the vessel wall in these tests. With the exception ofthe Si concentration (<0.1 ppm), this water chemistry is a good simulation of the ionic and
dissolved-gaseous species in J-13 water, although the pH25oc values are still somewhathigher than the reported near-neutral value for J-13 water. This, in part, can be attributedto some loss of CO2 to the gas phase above the water (i.e., air entrapped by a snug metal lidthat fits on top of the test vessel) at ambient pressure. The effluent water analyses fromtests W-10/W-23 indicate that the feedwater can be made up in a reproducible manner.
Beginning with test W-10, a pH electrode was incorporated into the test vessel toobtain in-situ values at the test temperature of 93°C. The measured pH values at 25 and
93°C are given in Table 21. Average values of the measured effluent pH25oc and the pH93oc
in the vessel for tests with the same feedwater chemistry (W-10/W-23) were 8.2 and 7.0,
respectively, or approximately one pH unit on the basic side of neutral at the twotemperatures. The pH25oc values in tests W-l/W-9 encompass the range of =7.3 to 9.2, orapproximately one pH unit on either side of the 8.2 value for the water chemistry that wasused in the majority of the SSRTs.
3.5 Measurement of Electrochemical Potential
The ECP of the insulated SSRT specimens was measured against an external 2 x 10--4M KCI/AgCI/Ag reference electrode at regular intervals during the test. Beginning withtest W-19, a small rod of the container alloy and a Pt wire were also inserted into the testvessel to obtain an independent measure of the ECP of the material and the Pt, as well as of
the SSRT specimen and the Ni vessel. The values for each electrode were plotted versustime, and the steady-state ECP values obtained from the plots are given in Table 22.Typical plots of the measured ECP of the SSRT specimens versus time are shown in Fig. 54for Incoloy-825 and the Cu-6% Al alloy in tests W-13 and W-15.
The measured values were also converted to the SHE scale. The SHE conversion
potential for an external AgCI/Ag reference electrode at 93°C as a function of KCIconcentration is shown in Fig. 55 and was obtained from relations for the thermocell andliquid Junction potentials. The calculated value for an electrolyte concentration of 2 x 10-4M (obtained from the figure) is +365 mV. An experimental SHE correction potential of
+378 mV for this electrode was obtained against a commonly used AgCl/Ag referenceelectrode with KCI electrolyte concentration of 0. I M. The latter value was used to convertthe steady-state ECP values in Table 22 to the SHE scale. The influence of temperature onthe SHE correction potential for the 2 x 10- 4 M KCI/AgCI/Ag reference electrode was alsocalculated, and the result is shown in Fig. 56,
The results in Table 22 indicate that the ECP values for the SSRT specimens rangefrom =230 to 310 mV(SHE) for Cu and Cu-base alloys and -_320 to 390 mV(SHE) for the
=
austenitic stainless steels and Incoloy-825 in nominally the same water chemistry (testsW-10/W-23). A comparison of these values with results for the con'esponding alloys intests W-l/W-9 indicates that the ECP values are not strongly dependent on the water
chemistry of these experiments. The ECP values of electrodes fabricated from the samematerials as the SSRT specimens are also shown in Table 22 fox"tests W-19/W-23. The
" ECP values of the unstrained austenitic steel electrodes are lower by _ 100 mV than those
i of the SSRT specimens (strained electrodes).
![Page 66: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/66.jpg)
58
Table 21. pH25°C of EJJluent Wa_er IOO ....... °.. ..... ,...-_",',-r-,",'_and pH93°C in Vessel
during SSRTs in soSimulated J-13 Water a E a
o =° °Test pH at pH at ¢.) _No. 25oc 93oc b m
m -50 aNCO
W-1 9.21 - >,
W-2 7.82 - _o .I00W-3 7.35 - ooW-4 7.33 - c- .15o_ "W-5 7.32 -W-6 6.86 -
W-7 6.89 - -200 ....... *'' J .... ° ....... *' ''W-8 8.88 - 0 2 0 0 4 0 0 6 0 0
W-9 9.11 - Elapsed Time (h)
W-10 8.51 7.70 (a)W-I I 7.98 6.90
W-12 7.76 6.95 100 ...... .. , ....... i ....... , ' "_W-13 8.33 7,25W-14 8.34 7.10W-15 8.31 7,30 SOW-16 8.26 7.20 _"W-17 8.10 7,10 EW-18 8.39 7.15 "" 0W-19 8.36 7.25 ¢_¢.)W-20 8.24 7.30 uj
.50W-21 8.35 7°25W-22 8.31 6.95 Ne.
W-23 8.26 6.85 o I._ a a _ m¢l;=© rg aW-24 8.35 6.95 m -100 a cP _ _©©
W-25 8.18 6.90 < a©W-26 8.28 6.90 -150W-27 8.23 6.85W-28 8.12 6.80W-29 8.11 6.80 -200 ....... I ,, , .... * ....... i • ..W-30 8.22 6.85 0 2 0 0 4 0 0 6 0 0W-31 8.11 6.90 Elapsed Time (h)W-32 8.01 6.55W-33 7.97 6.35 (b)
a Water chemistries are given In Tables Fig. 54° Electrochemical Potential of (a)17-20; nominally the same concentra- Incoloy 825 and (b) Cu-7%Al Alloytions of ionic species were present in SSRT Specimens at 93°C versus an
Tests W-10 to W-33. External 2 x 10 -4 M KCL/AgCI/Ag
b Neutral pH at 93°C is 6.18. Reference Electrode as a Function of
Time during Tests W-13 and W-15
![Page 67: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/67.jpg)
59
Table 22, Steady-State Electrochemical Potential of Candidate Waste Container
Materials, Platinum, and Nickel Test Vessel during SSRTs in SimulatedJ-13 Watera at 93°C
. SSRT Specimen Electrode Platinum NickelTest ECP, D - ECP, _-- ECP, c ECP, c ECP, cNo. Material mV mY(SHE) mV(SHE) mV{SHE) mV(SHE)
W-1 In-825 --145 233 ....W-2 In-825 -125 253 ....W-3 Cu-30% Ni .....W-4 304L SS -68 310 - - -W-5 Ch -75 303 - - -W-6 316L SS -110 268 - - -W-7 Cu-6% Al -55 323 - - -W-8 Cu - 110 268 - -W-9 In-825 -88 290 - - -
W-10 Cu-30% Ni - 140 238 - - -W-11 C_ -95 283 .....W-12 f._ -70 308 ....W-13 In-825 5 383 - - -W-14 Cu-30% Ni -85 293 - - -W-15 Cu-6% Al -110 268 ....W-16 Cu-6% Al -90 288 - - -W-17 316L SS --15 363 - - -W-18 C_ -90 288 - - 322W-19 316L -5 373 263 393 308W-20 304L -35 343 253 398 312W-21 Cu-6% Al - 150 228 248 388 293W-22 In-825 -60 318 223 398 328W-23 304L I 0 388 238 468 278W-24 316L -5 373 378 418 303W-25 304L - - 268 443 308W-26 304L - 10 368 318 443 308W-27 Cu-30% Ni -110 268 263 468 318W-28 Cu-6% Al -120 258 263 458 308
° W-29 Cu-6% Al -125 253 263 423 308W-30 In-825 -50 328 203 428 308W-31 Cu-30% Ni -120 258 258 448 318
. W-32 In-825 - I0 368 208 478 323W-33 Cu-30% Ni - 120 258 263 473 328
_, a Water chemistries are given in Tables 17-20; nominally the same concentrations of
I ionic species were present in Tests W-10 to W-33.b Electrochemical potential of the electrically insulated CERT specimens measured
against a 2 x 10 -4 M KCI/AgCI/Ag reference electrode.
c Electrochemical potential COITected to the standard hydrogen electrode (SHE) scale
by the addition of +378 mV to the measured values,
!
![Page 68: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/68.jpg)
6O
400 -_"_ • • • • ,,,,i ", , , 'i",'_,,i • • _ • ,,-,i • "", • • ,,--
"" 350
EU.l
300
o4_
u 250
o
° 2O00
100 ' ' ' '-__ ' ...... . ......... . "''" . " " _ 010 4 10 3 10 2 10 1 10
KCI concentration (N)
Fig. 55. Potential for Converting ECP Measurements from anExternal Silver Chloride Reference (SHE} Scale as a
Function of the KCl Concentration from Relationsfor 7_ermocell and Liquid Junction Potentials
, , . 4, I " • '" , • 1 • i , , , I " " '" " --I ''-'__
A
Ev
"_ 45oe_
on
= 400o
0
m
rf)300 ..... ' ' " ° _ I ,_ _ , i i .... n ....
0 25 50 75 100 125
Temperature (°C)
F_g. 56. Influence of Temperature on the Potential .forConverting ECP Measurements with an External2 x 10 -4 M KCl/AgCl/Ag Reference Electrode to the
Standard Hydrogen Electrode (SHE)from Relationsfor Therm_ell and Liquid Junction Potentials
![Page 69: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/69.jpg)
61
4 Fracture-Mechanics Crack-Growth-Rate Tests
4.1 Experimental Procedures
Compact tension (CT) specimens of 25.4 mm thickness were machined from 25.4-mm--thick plates of Type 304I, SS (Heat No. V70200), Type 316L SS (Heat No. 16650), and
Incoloy 825 (Heat No. HH2125F). The materials were tested in the as-recelved mill-annealed condition without additional heat treatment. Elemental composition andmechanical properties of the materials are shown in Tables 2-9.
Side grooves having a semicircular cross section were cut into both sides of thespecimen to a depth of" 1.27 mm to restrict crack growth to a single plane. The design ofthe CT specimens is in accordance with the ASTM specification E399, 14 except fo: theside grooves and six small threaded holes on the front face for instrumentation, as shownin Fig. 57. The stress intensity factors were calculated according to ASTM specification E-399. The direction of crack extension was perpendicular to the short transverse thicknessdirection of the plates. Rolling direction of the plates was not provided by LLNL or thevendors. Metallographlc examination of the materials did not reveal any clues ibr rollingdirection.
The specimens were fatigue-precracked irl air at room temperature for a length of1.91 mm to introduce a sharp starter crack The initial machine notch measured from the
load line was 17.78 mm. An isosceles triangular loading waveform at a frequency of I-2 Hz,a load ratio R (a ratio of minimum to maximum load) of 0.25, an initial maximum stress
intensity of 16.1 MPa.m !/2 and a final maximum stress intensity of 17.5 MPa.m I/2 was usedfor precracking. This final maximum stress intensity value is 70% of initial peak stressintensity ibr the subsequent crack-growth-tests in a simulated J-13 well water.
The initial peak stress intensity value for the tests in the simulated J-13 well waterwas chosen to be about 25 MPa.ml/2. Welding residual stresses are the most important
driving force for cracks. Under these loads, the largest marginally detectable defects thatwould be created during the fabrication of a waste container would have associated stress
intensity values approximately half the value chosen for these tests, which provides someconservatism.
The CGR tests were performed in a 5-L nickel vessel with a once-through flow
system at a flow rate of 3 mL/min, under 1 atm pressure at 92-94°C. The vessel was nothermetically sealed. The simulated J-13 well water was prepared from deionized high-pu_'Ity water (resistivity >16 Mi'l.cm) and reagent-grade-purlty salts of CaS04, Ca(NO3)2,CaCI2, FeCl2, Li2SO4, MgS04, MnSO4, AICI3, Na2C03, NaHCO3, KHCO3, Na2SiO3, and HF.
H_gh-purlty mixed gas containing 20% 02, 12%CO2, and 68% N2 was used as a cover gas at3--.5 psig to maintain the desired dissolved O2 and HCO_ concentrations. Table 23 shows a
typical composl.tion of J-13 well water I and analysis results for the simulated test solutionused for the CGR t¢'_ts. The test solution is a good simulation of the ionic and dissolved
gaseous species in the J-13 well water, with the exception of the Si concentration. Si wasnot_ _dderl tn the te_t solution to avoid precipitation of silicate. _ilicates are commonlyused as corrosion inhibitors for low-.temperature appllcatlons,12.13 and it is considered
unlikely that sillcates would contribute to envirorcnentally assisted crack growth of the testmaterials. The higher PH25oc values for the effluent test solution are due to some loss of
![Page 70: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/70.jpg)
62
Table 23. Chemical Composition of J-13 Well Waterand Test Solution
J- 13 Test Solution
Species Analysis Feed Effluent
Composition(rag/L)
Ca II.5 I0.0- 11.3 I0.I- 11,5
Mg 1.76 1.71 - 1.78 1.72- 1,88Na 45.0 48.3- 48.8 50.2- 50.9
K 5.3 5.21 -- 5_26 5.32 - 5.44
Li 0.06 0.057 - 0,058 0.059 .- 0.060
Fe 0.04 <0.01 <0.01Mn 0.001 <0,01 <0.01
Al 0.03 <0. I <0. I
Si 30.0 a. b a. b
Cu b <0.01 <0.01
Ni b <0.02 1,61- 4,66
F'" 2. I 2,02 - 2.10 2.03 -- 2.16
CI- 6.4 6.68 - 6.94 6.75 - 7.21
SO42- 18. I 19.3 - 20.5 20,4 - 20.9NO3- 10. I II.7 - 12.7 12.7 - 13,1
HCO_ 143,0 127 - ,129.5 132.2 - 14].Dlss. O 5.7 7 - 9 3.5 - 7
pH25oc 6.9 6.21 -6.81 7.71 - 9.31
aNot added.
bNot analyzed.
CO2 to the atmosphere during the tests, Nickel in the effluent is present primarily in the
form of corrosion products from the nickel test vessel.
The specimens and the platinum electrode were electrically insulated from the testvessel and load train. The corrosion potential of the specimens and a platinum reference
electrode with respect to an external 2 x 10 -4 M KCI/AgCI/Ag reference electrode were
measured ¢ <)ntmually during the crack growth tests. The potential of the reference
electrode at 93°C was experimentally determined to be +378 mV SHE. as discussed in
Section 3.5 and shown m Fig. 55. The corrosion potential varied from 376-431. 345--433,
337-403. and 39_497 mV SHE for the Type 304L SS, Type 316L SS, and Incoloy 825
specimens and the platinum electrode, respectively.
_ TPnQinn-tr_tpn_Inn lnnd.q were annlied to sDecimens with either MTS servohvdraullc
equipment under load--control or deadload testing machines. A sawtooth cyclic load_ waveform with variable rise and unloading time was used at a fixed R. Both hlgh-load-ratlo
(R _ 0,9) and low-load-ratio (R = 0,5 or 0,7) tests were conducted; the test conditions are__m:,|
:|-j-l
![Page 71: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/71.jpg)
63
i _+.o15 +.o2oI
----"--- 2,500 +,020 _ #29 (,136) DIA, 11/16 DP. ,,4t- 1.000--i1_#8-32 UNC-2B TAP .515 DP,+ /-.010 / 2 HOL"S
t
SURFACE "A" | _. .315-----I_ t
SPEC,MEN,D | L r-o,,-*-.°'° _5,,--_ J/,%W. I_ _
/_,_-_1.,./_r-S URFAC E "A" J 4.010 . " A--"( ._t_|_--.__/L______ 1.2oo-' ._ i
o ----,',,,,..;....,/Vi t ±o.,oI2.0 / l ,"' ,,_ A,: ._,o .
I
-- ----= , =- _-+0_o-_---
..o.,c. ,oo
"¢""_1 .,..olo '• .__=_=---_"--.soo".oooo,_. T
lr XXX-X![ II II I IIII Inll ' I I I' l o071
.o01,., DETAIL 'C' DETAIL 'l_,.,....,..,,.m' _---.13e
,-_ "--_ - ,: _ _qi_276...338_'--
1 ,047 R r7_l
....... : J (.10_) DIA. DRILL 11/16 DI'.#6-32 UNC-2B TAP .515 _+.015 L)P.
2 HOLES.
.047 .094 _ _ .050
LAY MARKS"roFALL----'"1 PERPENDICULARTO CENTER
SCALE: ! LINEOF RADIUS"MSURFACE"2".- 1"1 Tor_ _ oRBE_i i , ,,,,,, Hm ............
1. "A" SURFACES SHALL BE PERPENDICULAR WITHIN .004 TIR.2. THE iNTERSECTION OF THE NOTCH TIPS WITH THE TWO SPECIMEN FACES SHALLBE EQUALLY DISTANT
FROM THE TOP AND BOTTOM EDGES OF THE SPECIMEN WITHIN .010.
3. "M" SURFACES (SIDE GROOVES) AND NOTCH SHALL BE POSITIONED AS PER DRAWING # NW-O026A-W'2-FO.THIS ORIENTATION MUST BE 1DENT!FlED AT ALLTIMES DURING FABRICATION STEPS.
4. UNLESS OTHERWISE NOTED: FRACTtONALTOLERANCES+ 1/64: DECIMAL TOLERANCES +_,005 "
ANGULAR TOLERANCES +_1/4 o. FI_NISHTOLERANCES _ , ALL SURFACES TO BE FREE OF BURRS.
Fig. 57. Des_n of Compact Tension Crack-Growth-Rate Test Spectrnen.All dimensions ore in inches,
![Page 72: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/72.jpg)
64
summarized in Table 24. Three fatigue-precracked specimens were loaded simultaneously
in a dalsy-chain serial loading arrangement. The crack length in each specimen wascontinually monitored by means of a electric potential drop method.15 Potential drop
across the specimens was about 40--50 laV at a measuring current of 2 A, and thermalelectromotive force was on the order of 0.7-14 _LV. The resolution of the crack-length
measurement was 50 _tm. A schematic representation of the experimental setup Js shownin Fig. 58.
4.2 Results and Discussion
4.2.1 High-Load-Ratio Tests
Specimens of all three alloys were initially loaded under a constant (R = I) stressintensity of 25 MPa.ml/2 in the simulated J-13 well water environment, but no crackgrowth was observed after 315 h. The load ratio was than decreased to R = 0.95, thus
imposing a slight "wiggle" on the loading waveform, Out no crack growth was observed afteran additional 334 h under these conditions. Following this, R was further decreased to 0.9and the tests were continued for an additional 18,300 h {more than two yr), and again nocrack growth was observed. Figures 59-431 show crack length as a function of tlme for thetest times from 9300 to 19,000 h for the three alloys under R = 0.9 loading.
Table 24. Loading Conditions for eGR Tests onCandidate Waste Container Materials
Rise Unload
Kmu_'2_"l" Load Time TimeAlloy [MPa.m / ) Ratio (s) (s)
High..Load-Ratio Tests
All 2 5 1
All 25 0.95 12 2
All 2 5 0.9 12 2
Low-Load-Ratio Tests
304 SS 35.7 - 36.2 0.7 I - 500 127.4 - 28.5 0.5 I - 1000 I
316 SS 39.2 - 39.8 0.7 1 - 500 126.8 - 31.2 0.5 1 - 1000 1
Incoloy 36.4 - 36,9 0.7 I - 500 1825 27,4 - 28.3 0.5 1 - 500 I
![Page 73: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/73.jpg)
65
Load Reference
Electrode- r
,-" TO_; Drain
I.,._1
=._-]_Peristaltic _.
Pump |
Load63.mn',
_,, Tension
" Fig, 58. Schematic Representation of",,
Experimental Setup and TestSpecimen
The _naximum average crack growth rate in these tests can be estimated from theresolution of, the crack-growth-measurement technique (50 Ilm) and the time over whichno crack extension was detected. Dividing the overall resolution of 50 I_m by the testduration of ]9_000 h results in an estimated maximum crack growth rate of ==8x t0 "13 m/sunder the test conditions. This compares with a maximum allowable crack growth rate of
•, 1 x 10-12 m/s for the waste package canister, based upon a wall thickness of 1 cm and a
target life of 300 years.
4.2.2 _ow-Load-Ratlo Tests
Crack-growth-rate tests in the same environment, conducted under more severeconditions of greater stress intensities and lower R ratios, resulted in observable crackextension. In Fig. 62, Type 304L SS under conditions of R = 0.7, K = 36 MPa.m I/2, and
frequency of 0.5 Hz, shows a CGR of 4.0 x 10 -9 m.s -I. The results oi' cyclic load tests onTypes 304L and 316L SS and Incoloy 825 at R = 0.5 and 0.7 and frequencies of 10-3 to IHz are summarized in Table 25. For comparison, fatigue CGRs of austenitic stainless steel
in air at 93°C computed with the current ASME Section XI correlation, which is based onthe work of james and Jones, le are also included.
Figures 63 and 64 show a comparison between the CGRs observed for the testmaterials in simulated j-13 well water and the predicted growth rates of austenitic
:_| stainless steel in air, based on the ASME Section Xl correlation. In tl_e lIgures, growthI= rates on the solid line (with slope of unity) would be equal to those predicted by the ASME_|
-_ll
-I--m
![Page 74: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/74.jpg)
66
correlation. The observed CGRs for Types 304L and 316L SS and Incoloy 825 are generallylower than the predicted rates. Because the code correlation represents a 95% confidence
limit upper bound for the observed data base, it is expected to be conservative for mostheats of material in the absence of environmental effects.
Crack growth rate under cyclic loads in a corrosive environment (da/dt) may beexpressed as a sum of contributions by (I} stress corrosion cracking, (da/dt_scc;
(2) corrosion fatigue, (da/dt}cF, representing the additional crack growth under cyclicloading due to the environment; and (31 mechanical fatigue, (da/dt)alr, representing thefatigue growth in air:
(da/dt) = (da/dt)scc + (da/dt)cF + (da/dt)air. (20)
The first two terms on the right side of the equation are envlronment-sensltive.They depend on loading history variables, such as rise-, unload- and hold-time, as well as
on frequency. In oxygenated-water environments, the environment-sensitive terms cancontribute significantly to crack growth rates of austenitic stainless steels. 17-19 Underlow-R and high-frequency loading, mechanical fatigue dominates. Environmentalcontributions would be expected to become more significant as the frequency decreases.Crack-growth rates as a function of cyclic frequency and CGRs per cycle versus rise timefor the cun'c_nt tests are shown in Figs. 65-68. Figures 65 and 66 show that the time-based growth rates are proportional to frequency over the entire range of the frequenciesused in the tests. This indicates that no erwironmental acceleration of crack growth is
present for the test conditions considered. Figures 67 and 68 show that the growth rateper cycle is independent of rise time. This too indicates that no environmentally assistedcrack growth occurred, and that the crack-growth mechanism ts pure mechanical fatigue°For comparison, the environmentally accelerated behavior observed irl hlgh-temperatureoxygenated environments 18,19 is shown schematically by the curved lines in Figs. 65 and66.
5 Summary and Conclusions
A series of slow-strain-rate tensile tests on six candidate nuclear waste containermaterials was conducted under both crevice and noncrevlce conditions in simulated well
J-13 water at 93°C at strain rates of 10 -7 and 10-8 s-I. The tests were performed underwell-characterized environmental conditions. Similar tests were also performed on
weldment specimens of Types 304L and 316L SS, Incoloy 825, Cu, Cu-7%Al, and Cu-30%Ni at a strain rate of 10- 7 s-l The specimens contained small-dlameter
through-holes (with or without pins of a matching material) to facilitate observation of
cracks by scanning electron microscopy (SEM). The SEM observations showed cracking invirtually all of the materials under the severe testing conditions employed. A stress rat lowas formulated on the basis of the ratio of the increase in stress following the initiation of
local yielding for the material in water and the corresponding stress difference for anidentical test in air at the same elongation. A ratio of plastic strain in air to the plasticstrain in the environment (strain ratio), both evaluated at the same stress, was also
formulated to describe the cracking susceptibility. Higher values of stress or strain ratio
_ imply greater cracking or _¢_C susceptibtllty. Tile Stress or straln ratio appears to be uselulin screening the materials for SCC, even though the crack depths are small (<I00 _tm). On
ii-!
![Page 75: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/75.jpg)
67
Table 25, Cyclic CGRs, Obsen:ed and Calculated with ASME Section XI Correlation
Rise Kmax Observed ASME ,XILoad Freq. Time (MPa. Growth Rate Growth RateRatio (Hz) (s) ml/2) (m.s "'I ) (m's -I )
Type 304L SS
0.7 0.500 I 35.7 3.96 x 10-9 8.37 x 10 -90.7 0.167 5 35.9 1.62 x 10- 9 2.83 x 10-90.7 0.091 I0 36.0 7.64 x I0 -'Io 1.56 x 10 -90.7 0.048 20 36.0 4.41 x IO- Io 8.19 x I0 -lo0.7 0.020 50 36.1 2.31 x I0 -I0 3.39 x 10-1o0.7 0.010 100 36.1 9.73 x 10 -11 1.72 x lO-100.7 0.005 200 36.1 4.91 x I0 -ll 8.64 x I0 -110.7 0.002 500 36.2 2.29 x I0 -I I 3.48 x 10- II0.5 0.500 1 27.4 1.55 x 10- 8 1.59 x 10 -80.5 0.091 I0 27.8 2.15 x IO- 9 3.01 x 10-90.5 0.048 20 28.0 7.89 x 10-10 1.61 x I0 -90.5 0.020 50 28. I 3.96 x Io- lo 6.76 x 10-lo0.5 0.010 I00 28.2 1.78 x 10-10 3.46 x I0 -I00.5 0.005 200 28.3 9.40 x 10- I l 1.76 x I0 -100.5 0.002 500 28.4 3.94 x I0 -i I 7.14 x I0 -l I0.5 0.001 I000 28.5 1.95 x I0 -ll 3.59 x I0 -Ii
Type 316L SS
0.7 0.500 I 39.2 4.09 x 10- 9 I. 14 x 10 -80.7 0.167 5 39.4 1.93 x 10- 9 3.87 x 10 -90.7 0.091 10 39.6 9.66 x I0 -I0 2.13 x 10 -90.7 0.048 20 39.6 5.25 x 10-10 1.12 x 10 -90.7 0.020 50 39.7 2.06 x I0 -I0 4.64 x I0 --I°0.7 0.010 I00 39.7 6.81 x I0 -ll 2.35 x I0 -lo0.7 0.005 200 39.7 3.10 x I0 -ll 1.18 x I0 -l°0.7 0.002 500 39.8 1.82 x I0 -l I 4.76 x 10 -l l0.5 0.500 I 26.8 2.33 x IO- 8 2.02 x 10-80.5 0.091 I0 30.0 3.97 x IO- 9 3.88 x 10-.90.5 0.048 20 30.3 I. 12 x 10- 9 2. I0 x 10-90.5 0.020 50 30.6 5.65 x 10-10 8.91 x l0 -lo0.5 0.010 I00 30.8 2.69 x I0 -lo 4.60 x 10 -Io0.5 0.005 200 31.0 1.34 x I0 -lo 2.36 x I0 -'lo0.5 0.002 500 31. I 5.36 x IO- I I 9.58 x 10--I l0.5 0.001 I000 31.2 2.64 x I0 -II 4.84 x 10-11
Incoloy 825
0.7 0.500 I 36.4 4.89 x IO- 9 8.86 x 10- 90.7 0.167 5 36.6 1.56 x 10- 9 3.01 x 10- 90.7 0.091 I0 36.7 9.55 x I0 -I0 1.66 x 10-90.7 0.048 20 36.7 5_28 x 10-10 8.74 x I0 -lo0.7 0.020 50 36.8 1.60 x l0 -10 3.61 x I0 -lo0.'7 0.010 I00 36.8 9.73 x lO -II 1.83 x l0 -100.7 0.005 200 36.9 5.84 x I0 --I l 9.23 x 10-II0.7 0.002 500 36.9 2.62 x I0 -l I 3.72 x I0 --l I0.5 0°500 l 27.4 9.05 x IO- 9 1.58 x 10-80.5 0.091 I0 27.6 1.70 x 10- 9 2.96 x 10-9
i 0.5 0.048 20 27.8 7.04 x iO -10 1.58 _ 10--9
0.5 0.020 50 27.9 3.54 x 10-10 6.61 x 10-100.5 0.010 I00 28.1 1.67 x IO- I0 3.39 x I0 --lo0.5 0.005 200 28.2 1.22 x I0 -10 1.72 x I0 -l'00.5 0.002 500 28.3 3.88 x 10-1] 6.99 x I0 -I I
![Page 76: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/76.jpg)
68
19.7 , i" ' u , l , I , u ,m
m
mm
EE
19.6 w__===a_l_cG).J
19.5
u,
_" , I , I_ i I , .I ' 1 ....,,, ,,,
8,000 12,000 16,000 20,000
Test Time (h)
Fig. 59. Crack Length vs. Test Time for Type 304LSS at Kmax = 25 MPa.m I/2 and R = 0.9
19.7 ' I ' I ' n , -'f_- 'l • -
EE
.c:...19.6 _T_,_._,t_=_,q=_=_pO)t-
..I ,-m m
¢_ 19.5 -
,_ i I , ,,I . l__:J | , I l ....
8,000 12,000 16,000 20,000
TestTime (h)
Fig. 60, Crack Length vs, Test Time for T_.pe 316LSS at Kmox = 25 MPa.m 112 and R = 0.9
![Page 77: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/77.jpg)
69
' I " l-' ' I " I ' I "
19.5 i I , I , I i i , I ,8,000 12,000 16,000 20,000
Test Time (h)
P_j. 61. Crack Length vs. Test "f'bnefor Incoloy 825at K..nax= 25 MPa.m1/2 emd R = 0.9
22.4 . , .r- , '1 ' , .i , I ' ' ' ;-"
E
E j"" 22.3E ,,.
..I .--,,,=
i "_ 22.2 ,m
, , • _--u. , , [ i , , ,
14,635 14,640 14,645 14,650
TestTime (h)
Fig. 62. Crack Length us. 3"estTbne for 304L SS atKmex = 36 MPa.mI/2 R = O.7 and. 0.5 Hz
ii,,,i,, _,,,,, i, _.... II' _l,lr ','I,
![Page 78: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/78.jpg)
7O
10.7 "' , , Ill'i"_ I v'l IJdlrwI v wI,,_--I I wl_,,,_
o 3O.Lss_" o 316L SS _ -,,
_ 10.8 [" 13 Inc°l°y825 f "!-o,_ez::10-9 - -1=.-
_ 10.1o oQ
10.11 , , ,.A,li*l * , =,,=,,I * , ,,,,.I , , ,i,,,_10-11 10-10 10.9 10.8 10 .7
ASME AirCrackGrowthRate,daJdt(m/s)
P_j. 63. _e-_ed CGR vs. Rate for AusteniticStainless Steels in Air from ASME SectionXI Correlation for R = 0.5
10"7 ' '''""I _ '''""I r-r"vTr'"l ' ''_A
09 f0 304L SS /
_" 0 316L SS J'_10"8 "D Incoloya25 j'_. "_
"o
: 7"?30
f"9 0"10 f_O0'.L_1,... 1
10.11 , , ,,,,,,I I ! ,,j,,,i , I I,p,ul _._.._10"11 10"1° 10"° 10-8 10"7
ASME AirCrackGrowthRate, da/dt(m/s)
F_g. 64. Time-Based CGR vs. Rate for AusteniticStainless Steels in Air from ASME SectionXI Correlation for R = O.7
![Page 79: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/79.jpg)
71
lo_ r-
_ _ o 304L SS....sF <> 316LSS
# _,..__._....,.Z...._,_..¢.,_=0 -slope= I ,
10"10t_v_ronmenta'8 "I.
10"11k acceleration 1,_t,,.. Eo
I0-121 , i i =llli| , i i lll.ll | , , ill.
10.3 10"2 10 "1 100
Frequency(Hz)
Fig. 65. Time--Based CGR vs. Frequency at R = 0.5
107 " ' ' '''"'I , , r,,,,,I ' ' '"""
•_ o 304L SS_, 108 O 316L SS
. o incoloy825 ,=.j
lO'r ,, R_ __- "_", "l
slope=li.L9 ,""" "environmental"_ 10"11 I,_ acceleration .o
10.12 , . ,,,.,,I , , .,,,,,I , , ,,,,,,103 102 101 i 00
Frequency(Hz)
Frg. 66. T#ne-Based CGR vs. Frequency at R = O.7
![Page 80: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/80.jpg)
72
_m 10"5"-" '" w i w1,.l_ I'l ,llv.] " I I _,lll. I ¼ ! lVR,
o 304L SS
"_ 10.6 • 316LSS .._¢; o Incoloy825 !"O
o_ 10"7 . 1
O o a _ A A ,,. ,., ;10-8 .
10.r
10..10" , ,,_,l,.I , i ,,il,,I , ,l,iu, I , ,,,ii,0"1 100 101 102 103
Rise Time (s)
l_g. 67. CGR per Cycle as a Function of Rise Timefor R = 0.5
'-'_ 10"51 i w Vllw. I , ,"wyhl,, I i I,"',,iw_, I'' w d"'l,,'lt
o 304L SS"_ 10.6 _' 316LSS"-" r a IncoloyU25tO ,-
>., 0.7£ 1 r
i lo-8(.9 10"9tO
I
O 10.10 I ,,,,,,J , i,,,i.l , , ,,..I , iº,i.,II0"I 100 101 102 103
Rise Time (s)
_g. 68. CGR per Cycle as a Function of Rise Time forR=0.7
ii
I_q ....... ' .... IPlr_J J4"_1 "" 'h' II'IWll " _'_' '
![Page 81: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/81.jpg)
73
the basis of this stress ratio or strain ratio, the ranking of the materials in order of
increasing resistance to cracking is Type 304L SS < Type 316L SS < Incoloy 825 < Cu-30%Ni < Cu and Cu-7%A1. Weldment specimens of Cu-30%Ni and Cu exhibited a
somewhat higher susceptibility to cracking in terms of the index compared to the basemetal specimens. The cracking index also suggests that a lower strain rate has adeleterious effect on cracking of types 304L and 316L FS, Incoloy 825, and Cu, but has
virtually no effect on Cu-30°/oNi and Cu--7%AI. The relative SCC susceptibility of thesematerials from the preliminary SSRT tests is bei:lg confirmed by tests on fracture-mechanics-type specimens.
Fracture-mechanics crack-growth tests were conducted on 25.4--mm-thick
compact tension specimens of Types 304L and 316L SS and Incoloy 825 at 93°C and1 atm of pressure in simulated J-13 well water in both high- and low-load-ratio tests. Inthe high-load-ratio tests, Kmax was 25 MPa.m 1/2 and R ranged from 0.9 to 1. In the low-load-ratio tests, Kmax ranged from 26.8 to 39.8 MPa.m 1/2 and R was 0.5 or 0.7. The resultsof these experiments lead to tile following conclusions: (1) No crack growth was detectedin any of the alloys tested at K = 25 MPa.ml/2 and R = 0.9-1 for test times of 19,000 h.Based on the resolution of the crack-length-measuring technique, this indicates that the
maximum average crack growth rate under these conditions was =,8 x 10 -13 m/s. (2} No
cyclic or rise-time-dependent environmental acceleration of crack growth was observablein the simulated J-13 well water at 93°C under the test conditions. (3) Growth rates for R= 0.5-0.7 and maximum stress intensities of 26-40 MPa.ml/2 agree with the current ASMESection XI correlation for austenitic stainless steel within a factor of 0.9-3.8.
Acknowledgments
D. R. Perkins, W. F. Burke, W. E. Ruther, W. K. Soppet, S. L. Phillips, and J. C. Tezak of
Argonne National Laboratory contributed to various experimental aspects of the project. E.A. Huff, A. M. Essllng, and F. P. Smith analyzed the water from the SSRT tests. The authorsthank W. L. Clarke and R. D. McCright of Lawrence Livermore National Laboratory for their
support of t riis work, which was sponsored by the U.S. Department of Energy undersubcontract from Lawrence Livermore National Laboratory.
References ...... _
I. R.V. Guzowski, F. B. Nimick, M. D. siegel, and N. C. Finely, Repository Site Data
Report for Tuff: Yucca Mountain, Nevada, NUREG/CR-2937, SAND82-2105, SandiaNational Laboratories (Oct. 1983).
2. A.E. Ogard and J. F. Kerrisk, Groundwater Chemistry along Flow Path Between aProposed Repository Site arid the Accessible Environment, LA-1088-MS, LosAlamos National Laboratory (1984).
3. J.C. Farmer and R. D. McCright, A Review of Models Relevant to the Prediction of
Perjormance of High-Level Radioactive Waste Disposal Containers, CORROSION 89,New Orleans, Paper 519, National Association of Corrosion Engineers, Houston
(1989).
!1[I ,, "'" "' Iii' '" ' r,lFill,, I, ........ I,illlllll"ll" F'li I,,, lr, ' '1.... II I1?1' ii' ' _nrlll Iliil'_lnl, llrn_
![Page 82: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/82.jpg)
74
4. R.D. McCright, FY 1985 Status Report on Feasibili_. Assessment of Copper-Base
Waste Package Container Materials in a Tuff Repositonj, UCID-20509 DE86003960,
Lawrence Livermore National Laboratory (Sept. 30, 1985).
5. P.S. Maiya, Constant Extension Rate Tests, in Environmentally Assisted Crackin_ _
Light Water Reactors: Semiannual Report April-September 1986, NUREG/CR-4667,
Vol. III, Argonne National Laboratory Report ANIr87-37 (Sept. 1987).
6. P.S. Maiya, Effects of Plastic Strain, Environment, and Crevices on Stress Corrosion
Crack Iniiiation and Propagation in Types 316NG and 304 Stainless Steel Corrosion,
45, No. 11, pp. 915-914 (1989).
7, W. Ramberg and W. R. Osgood, Description of Stress-Strain Curves by ThreeParameters, NACA Technical Note No. 902 (July 1943).
8. H. Neuber, Theory oJ" Stress Concentration for Shear Strained lh-ismatical Bodies
with Arbitrary Non-linear Stress-Strain Law, ASME J. Appl. Mech., 28, pp. 544-550(1961).
9. P.S. Malya and W. J. Shack, Evaluation oJ"Nonenvlronmental Corrective Actions, In
Environmentally Assisted Cracking in Light Water Reactors: Annual Report October
1982-September 1983, NUREG/CR-3806, Argonne National Laboratory Report ANIr
84--36, p, 58 (June 1984).
10. W.J. Shack, private communication, Argonne National Laboratory (1990).
11. R.K. Uer, The Chemistry of Silica, John Wiley & Sons, New York, pp. _'Y-59 (1979).
12. H.H. Uhlig, ed., Corrosion Handbook, John Wiley & Sons, New York, pp. 500--503(1948).
13. R.T. Hanlon, A. J. Steffen, G. A. Rohlich, and L. H. Kessler, Sca/e and Corrosion
Control in Potable Water Supplies at Army Posts, Ind. Eng. Chem., 37, 724-735(1945).
14. Standard E 399-83, Standard Test Method for Plane-Strain l_'racture Toughness of
Metallic Materials, in Annua I Book of ASTM Standards, Vol. 03.01, Amellcan Societyfor Testing and Materials, Philadelphia, pp. 487-511 (1989).
15. T.A. Prater, W. R. Catlin, and L. F. Coffin, Environ,"nental Crack Growth
Measurement Techniques, EPRI NP-2641, Electric Power Research Institute, Palo
Alto, CA (1982).
16. L.A. James and D. P. Jones, Fatigue Crack Growth Correlation for Austenitic
Stainless Steels in Air, Proc. Conference on Predictive Capabilities in
EnvironmentaUy-Assisted Cracking, R. Rungta, ed., PVP Vol. 99, American Society
of Mechanical Engineers, New York, pp. 363-414 (1985),
![Page 83: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/83.jpg)
75
17. T. Kawakubo, M. Hishida, K. Amano, and M. Katsuta, Crack Growth Behavior of
T_l.pe 304 Stainless Steel in Oxygenated 290°C Pure Water under Low Frequency
Cyclic Loading, Corrosion, 38, 638-647 (1980).
18. J.D. Gilman, R. Rungta, P. Hinds, and H. Mindlan, Corroslon-Fatigue Crack Growth
Rates in Austenitic Stainless Steels in Light Water Reactor Environments, Int. J.
Pres. Ves. & Piping 31, 55-68 (1988).
19. W.J. Shack, Corrosion Fatigue Curves for Austenlttc Stainless Steels in Light Water
Reactor Environments, in Envlrom'nenlally Assisted Cracking in Light Water
Reactors, Semiannual Report, October 1990-March 1991," NUREG/CR-4667,
Vol.12, Argonne National Laboratory Report ANL--91/24, pp. 30-36 [Aug. 1991).
![Page 84: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/84.jpg)
]p___trlbutlon for ANI_92128
d. K. Bates T. Jennings R.B. Poeppel
S. S, Bm'ys T.F. Kassner D.T. ReedK. Brubaker P.S. Malya W.E. RutherJ. C. Burton C.A. Malefyt (2) W.J. Shack
O. K. Chopra V.A. Maroni W.K. SoppetJ. C. Cunnane Z. Nagy C.E. TillD. R. Dlercks K. Natesan R.W. Weeks
J. D. Dltmars L. A_ Neimark ANL Patent Dept.W. Harrison j.Y. Park (501 ANL Contract FileA. B. Hull P.J. Peterson TIS Files 13}
DOE--OSTI for distribution per UC-504 and UC-510 (2.37)ANL-TIS Libraries
Chicago Operations Office, DOE:D. T. Goldman
F. HerbatyA. L. Taboas
Materials and Components Technology Division Review Committee:
H. Berger, Industrial Quality, Inc., Gaithersburg, MDH. Blrnbaum, University of Illinois at Urbana-Champaign, UrbanatL Buchanan, University of Illinois at Urbana-ChmT-_,patgn, brbanaM. S. Dresselhaus, Massachusetts Institute of Technology, Cambridge, MA
R. A. Grecnkom_ Purdue University, West Lafayette, IN
B. Jones, University of Illinois at Urbana-Champaign, UrbanaC.-Y. Li, Cornell University, Ithaca, NYIL E. Smith, Electric Power Research Institute, NDE Ctr., Charlotte, NC
W. L. Clarke, Lawrence Livermore National Laboratory
J. IL Crttrn, INCO Alloys Intematlonal, Huntington, WV
J. H. DeVano Oak Ridge National Laboratoryj. N, Kass, Lawrence Livermore National Laboratory
W. S. Lyman, Copper Development Association, Inc., Greenwich, CTR. D. McCright, Lawrence Livermore National LaboratoryM. A. Molecke, Sandia National LaboratoriesE. Smaflos, Kernforschungszentrum Karlsruhe, Karlsruhe, FRG
R. Van Konyenburg, Lawrence Livermore National LaboratoryR. E, Westerman, Baflelle Pacific Northwest LaboratoriesB. E. Wilde, Ohio State University, Columbus.
![Page 85: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/85.jpg)
![Page 86: STRESS CORROSION CRACKING OF CANDIDATE WASTE CONTAI …/67531/metadc625520/... · ARGONNE NATIONAL LABORATORY ANL-92/28 9700 South Cass Avenue, .Argonne, lUinois 60439 Distribution](https://reader033.vdocument.in/reader033/viewer/2022060803/60876e7cb65d5553255e0d27/html5/thumbnails/86.jpg)