![Page 1: Welding Procedure Specification QW-482portal.tmcorp.us/ManagerDocs/CodeWeld/WPS-JTT-24-PWHT.pdfQW-482 WELDING PROCEDURE SPECIFICATION (WPS) Company Name: By: ... ular form similar](https://reader036.vdocument.in/reader036/viewer/2022082216/5afd6dc87f8b9a994d8d7a1c/html5/thumbnails/1.jpg)
QW-482 WELDING PROCEDURE SPECIFICATION (WPS)
Company Name: By:Welding Procedure Specification No.: JTT-24-PWHT Revision No. 0 Date: 7/6/2009Supporting PQR No.(s) JTT-24-PQR (PWHT) Revision No. 0 Date: 7/6/2009Welding Process(es) Type(s)
(Automatic, Manual, Machine, or Semi-Auto.)
JOINTS (QW-402) DetailsJoint DesignBacking (Yes) (No)Backing Material (Type)
(Refer to both backing and retainers.)
Metal Nonfusing MetalFillet weld
Nonmetallic Other See Project Specifications
Sketches, Production Drawings, Weld Symbols or Written DescriptionShould show the general arrangement of the parts to be welded. Whereapplicable, the root spacing and the setails of weld groove may bespecified.
(At the option of the Mfgr., sketches may be attached to illustrate jointdesign, weld layers and bead sequence, e.g. for notch toughness proce-dures, for multiple process procedures, etc.)
* BASE METALS (QW-403)P-No. Group No. to P-No. Group No.
J.T. Thorpe & Son, Inc. J. Jacob Dupree, P.E., Q.C. Manager
SMAW Manual
4 8
FilletN/A
N/A
P No. Group No. to P No. Group No.OR
Specification Type and Gradeto Specification Type and Grade
ORChem. Analysis and Mach. Prop.to Chem. Analysis and Mach. Prop.Thickness Range:
Base Metal:Pipe Dia. Range: Groove FilletOther
* FILLER METALS (QW-404)Spec. No. (SFA)AWS No. (Class)F-N0.A-No.Size of Filler MetalsWeld Metal
Thickness Range:GrooveFillet
Electrode - Flux (Class)Flux Trade NameConsumable InsertOther
*Each base metal - filler metal combination should be recorded individually.
N/AN/AN/A
43
3/32", 1/8", 5/32"
N/AAny size fillet weld
N/A
4 8
1060 Hensley Street, Richmond, CA 94801tel: 510-233-2500 fax: 510-233-2901
www.jtthorpe.com
5.11
Any thickness base metalAny size fillet weld
ENiCrFe-3 (INCO 182)
![Page 2: Welding Procedure Specification QW-482portal.tmcorp.us/ManagerDocs/CodeWeld/WPS-JTT-24-PWHT.pdfQW-482 WELDING PROCEDURE SPECIFICATION (WPS) Company Name: By: ... ular form similar](https://reader036.vdocument.in/reader036/viewer/2022082216/5afd6dc87f8b9a994d8d7a1c/html5/thumbnails/2.jpg)
QW-482 (Back)WPS No. JTT-24-PWHT Rev. 0
POSITIONS POSTWELD HEAT TREATMENT (QW-407)Position(s) of Groove N/A Temperature Range
Welding Progression: Up Down Time RangePosition(s) of Fillet
GAS (QW-408) NonePREHEAT (QW-406) Percent Composition
Preheat Temp. Min. Gas(es) (Mixture) Flow RateInterpass Temp. Max.
Preheat Maintenance Shielding N/A N/A N/A(Continuous or special heating where applicable should be recorded) Trailing N/A N/A N/A
Backing N/A N/A N/A
ELECTRICAL CHARACTERISTICS (QW-409)Current AC or DC DC Polarity DCEPAmps (Range) Volts (Range)
(Amps and volts range should be recorded for each electrode size,position, and thickness, etc. This information may be listed in a tab-ular form similar to that shown below.)
Tungsten Electrode Size and type(Pure Tungsten, 2% Thoriated, etc.)
Mode of Metal Transfer for GMAW(Spray arc short circulating arc etc )
1250°F - 1350°F1 hour minimum
40 - 125 20 - 30
X
None 350°F
None required
N/A
N/A
ALL
(Spray arc, short circulating arc, etc.)
Arc Timing
TECHNIQUE (QW-410)String or Weave BeadOrifice or Gas Cup Size N/AInitial and Interpass Cleaning (Brushing, Grinding, etc.) Grinding and Brushing
Method of Back Gouging N/AOscillation N/AContact Tube to Work Distance N/AMultiple or Single Pass (per side)Multiple or Single ElectrodesTravel Speed (Range)Peening No peening
Other(e.g., Remarks, Com-
Travel ments, Hot WireWeld Type Amp. Volt Speed Addition, Technique,
Layer(s) Process Class Dia. Polar. Range Range Range Torch Angle, Etc.)
SMAWSMAWSMAW manual
Any layerAny layerAny layer
DCEPDCEPDCEPENiCrFe-3
40 - 6565 - 95
95 - 125
20 - 2521 - 28ENiCrFe-3
ENiCrFe-3 3/32"1/8"5/32" 22 - 30
manualmanual
N/A
www.jtthorpe.com
Filler Metal Current
1060 Hensley Street, Richmond, CA 94801tel: 510-233-2500 fax: 510-233-2901
String or weave
SingleSingle or multiple
Manual
![Page 3: Welding Procedure Specification QW-482portal.tmcorp.us/ManagerDocs/CodeWeld/WPS-JTT-24-PWHT.pdfQW-482 WELDING PROCEDURE SPECIFICATION (WPS) Company Name: By: ... ular form similar](https://reader036.vdocument.in/reader036/viewer/2022082216/5afd6dc87f8b9a994d8d7a1c/html5/thumbnails/3.jpg)
QW-483 PROCEDURE QUALIFICATION RECORD (PQR)(See QW-200.2, Section IX, ASME Boiler and Pressure Vessel Code)
Record Actual Conditions Used to Weld Test Coupon
Company Name: J.T. Thorpe & Son, Inc.Procedure Qualification Record No.: JTT-24-PQR (PWHT) Rev. 0 Date:WPS No. JTT-24Welding Process(es) SMAWTypes (Manual, Automatic, Semi-Auto.) Manual
JOINTS (QW-402)
Groove Design of Test Coupon(For combination qualifications, the deposited weld metal thickness shall be recorded for each filler metal or process used.)
BASE METALS (QW-403) POSTWELD HEAT TREATMENT (QW-407)Material Spec. SA-387-11 Cl.1 & 2 to SA-240-304 Temperature 1250 °FType or Grade Time 1 hourP-No. P-4 to P-No. P-8 Other N/AThickness of Test Coupon 1/4" plate x 1/4" plate
24-Jun-09
¼” SA-240-304LPlate
¼” SA-387-11 Cl. 2 plate
¼” fillet weld (typical both sides) E-309L-16
¼” SA-240-304 Plate
¼” SA-387-11 Cl. 1 & 2 plate
¼” fillet weld (typical both sides) ENiCrFe-3 (INCO-182)
Thickness of Test Coupon 1/4 plate x 1/4 plateDiameter of Test Coupon N/AOther
GAS (QW-408) NonePercent Composition
Gas(es) (Mixture) Flow RateShielding N/A N/A N/ATrailing N/A N/A N/A
FILLER METALS (QW-404) N/A Backing N/A N/A N/ASFA Specification 5.11AWS Specification ENiCrFe-3 (INCO 182) ELECTRICAL CHARACTERISTICS (QW-409)Filler Metal F-No. Current DCWeld Metal Analysis A-No. Polarity ReverseSize of Filler Metal 1/8" Amps. 85 - 90 Volts 23 - 25Other Tungsten Electrode Size N/A
OtherWeld Metal Thickness 1/4"
POSITION (QW-405) TECHNIQUE (QW-410)Position of Groove Flat Travel SpeedWeld Progression (Uphill, Downhill) N/A String or Weave Bead weaveOther Oscillation N/A
Multipass or Single Pass (per side) single passSingle or Multiple Electrodes single
PREHEAT (QW-406) OtherPreheat Temp. 350°FInterpass Temp. Single pass (no interpass temp.)Other Sample air cooled after welding
1060 Hensley Street, Richmond, CA 94801tel: 510-233-2500 fax: 510-233-2901
www.jtthorpe.com
43
¼” SA-240-304LPlate
¼” SA-387-11 Cl. 2 plate
¼” fillet weld (typical both sides) E-309L-16
¼” SA-240-304 Plate
¼” SA-387-11 Cl. 1 & 2 plate
¼” fillet weld (typical both sides) ENiCrFe-3 (INCO-182)
![Page 4: Welding Procedure Specification QW-482portal.tmcorp.us/ManagerDocs/CodeWeld/WPS-JTT-24-PWHT.pdfQW-482 WELDING PROCEDURE SPECIFICATION (WPS) Company Name: By: ... ular form similar](https://reader036.vdocument.in/reader036/viewer/2022082216/5afd6dc87f8b9a994d8d7a1c/html5/thumbnails/4.jpg)