OW-482 SUGGESTED FORMAT FOR WELDING PROCEDURE SPECIFICATION (WPS)
tsee OW-201 .f , Sultion lX' ASME Boiler and Pressure Vessel Code)
companyNameWoodlandEnterprise.!,9ox718-.SpiritRiver,AlbeJrlalO!9908y:PeterWoodcock,C'E.T.wetding Procedure specf il'r-lng Fon Nlo (s) 01s' o2s' 03s' 04s' 05s
Revision No. o Date o
wJaing P..ufu0., inutorn.tic, ufanttaf , l''facnine' Semi-Auto') Manual
JOTNTS (OW402)Joint Design See attacneo (All A D IM'
ALBERTA BOILERS SAFE.
PRO\/INCE CF r.uL ;'r',
SAFETY CODES i:TWELDING PRCCEDuT::i
No VrrP.......... .....?,?.-l V' .2.
Backing (vesil rq ttlo) L-13---:--:-Backini irr.turi.t 1fyp.) Weld metal where aqpliqaFle "
(neter to Ootn backing and retainers)
(No Retainers)
ID
Metal
Nonmetallic
Nonfusing Metal
Other
trtr
Reg.
Spec
w6ld
r.!o ....................W.8.:..Q.?proce::.. ..................5..{?.+..W
Sketches, Production Drawings, Weld Symbols or Written
Description should show the goneral arrangement of the
parts to be welded. Where applicable, the root spacing
and the details of weld groove may be specified'
(At the option of the Mfgr', sketches may be attached to
illustrate joint design, weld layers and bead sequencs'
e.g. for notch toughness procedures, for multiple Process
procedures, etc.)
'BASE METALS (OW4O3)
P-No. 1 GrouP No'
OR
Speciflcation tYPe and grade
to Specification tYPe and grade
OR
1 &2 to P-No. Group No 1&2
Chem. AnalYsis and Mech' ProP'
to Chem. AnalYsis and Mech, ProP'
Thickness Range: '2'7 mm to 25'4 mm
Base Metal: oiooue 0,1185"to 1,0' :iP].+l#*T=
Other' (lmoact tested
odrs rvrero''
-
Fillet All rhicknessPipe Dia. Range: Groove All Dia' . ..-..
No weld oass to exceed 1/2"'
'FILLER METALS (OW4O4)
Spec. No. (SFA)
AWS No. (Class)
Groove (MAX)Fillet
Electrode-Flux(Class)Flux Trade Name
Consumable lnsertOther
. E".h b.r" r.t"t-ntlur m"Ill-bination should be recorded individually'
QW482 (Back)
WPS No. WE-02 Rev. 0
POStTtONS (QW-405)Position(s) of Groove AllWeldingProgression: @
POSTWELD HEAT TRE.ATMENT (QW-407)Temperature Range 1
.1 25. F +A 25. FTimeRange txourffi
PREHEAT (OW - 406)Preheat Temp. Min 500.FlnterpassTemp ru"r@Preheat Maintenance Gas or Electric(continuous or rp""i"rffirecorded)
GAS (QW-408)
Percent ComposjtionGas{es) Mixture Flow Rate
N/A
ELECTRTCAL CHARACTERtsTtcs (ow-409)Current AC or DC DC polarity Rev Maximum Heat lnput
ilH"T:i3:,n",.^g * -Yolts
tnans";t l7-?3 51,000 Joures (ALL TH,ckvEss RAvGEs(Amps and volts range should be recorded toi eaci "te.troolffiosition, "no"tni"c"x"n;:::""1.
t
fi;information may be listed in a tabular form similar to that shown below.)
Tungsten Electrode Size and Type
Mode of Metal Transfer for GMAW
Electrode Wire feed speed range
(Pure Tungsten, 2% Thoriated, etc.)
(Spray arc, short circuiting arc, etc)
TECHNTQUE (OW41O)String or Weave BeadOrifice or Gas Cup Size N/Alnitial and lnterpass Cleaning (Brrs
Contact Tube to Work DistanceMultiple or Single pass(per side)
Travel Speed (Range)
Other (e.9., Remarks,Comments, Hot WireAddition, Technique, TorchAngle, Etc.)
SEEATTACHED
PneHEAT
A.
C.
D.
E.
We1ds joining pressure partspreheated to not less than thestated in F.
of attachmentsmininum preheat
shaLL betomnor>rrrF6
The preheat temperature sha11cornpleted.
If welding is inter:rrpted, theshall be re-heated to sthespecified in F.
be naintained until welCrng
weld joint and adjacenr areasroininum preheat temperacure
The preheated area sharr not be ress than 5o.B rnmwide on each side of the weld.(2 rn.)
Preheat temperatures sha]1 be checkedinspector, using temperature ind.icatingreputable nethods.
by the welde:- c:crayons or othe:-
F. Mj-nimum preheating ternperatures sharr be as forrows:
1. Pnessune Vgssels
Nouin l lyal1 Tbickness Hinimurn Preheat Temperature
0 to 25.4 nm (0 to 1in.)over 25.4 ur:n to 203 r'h (over 1 to B in. )
over zs.A Yn'n ( 1. o in. ) when trax.carbon content exceeds O.3O*
f n.- / c^.F\rv ! ( JU : )
94'C (200.F)
B0'c (17s.F)
2.tlrrx ANSI 831. 3
Nominal lfallTbickness
<25.4 mm ( 1.0 in)>ZS .4 mrn ( 1. 0 in. )
AlI
REpTNERY
Xiu. SPecified Teusi'IeStrenqtb, Base Hetal
S49O mPa (7I Ksi)AlI
>490 mPa (72 Ksi)
ru AccoRDANc E
Xininum PrebeatTe!]perature
lo'c ( 50'F)an.- /'t?q'F\ev v \-,J - l
on.a /'?q'F\9W v \-i J
3.
Nominal I{aII Tbic)<ness
>25.! :um ( 1. o in. ) when
Carbon content exceedsAII others
llinimum Prebeat TemPerature
B0'c (r.75'F)
1n.^ / =^t:\MIJv:)
naxl-I!um
0.30t
PosrwELD Henr TnEaTMENT
Postweld Heathowever, vhen
Treatuent isrequired the
not mandatory for all thicknessesfollowj.ng sha}I apply:
1. R ANCE lll ASME VIII DrvrsroN1, UW-40 & ucs-s5
Holdlne Teuxperature
595 co 550'(f100 co 1200'F)
Nores:
Eoldlng Tfune, Based onUp to 50.8 rnn (2 ln.\
15 ninuces minimum,t hr, per 25.4 rnn (fn. )
Nomlnal IJaII Th !ckrre s s
Over 50.8 rnm (2 in )
2 hr. plus I5 ninucesfor each aCC:-cionai
25 .4 m.o, ( in I ove:50.8 ur,r (: in .,
38.1 nun (Ii in.).
over 31.8 rrun (li( 1\ in. ) when a
applied.
L. PWHT is nandatory on material_ over
2. PWHT is not rnandatory on u.raterialin.) up to and including 38.1 rnrlnrinimun preheat of 93 . C ( 2 OO . F) is
2. 9HEMTcAL ?LANr & PernoueuN Rerrxrnv Prprxc rN AcconoaNce l,lrrHANSI 831.3
Norolnal ValI ThtcknessOver I9.l mm (i ln )
I h:. n!nimu-nI hr. per 25 .4 nm ( in. )
3.
Holdtns Temoereture
595 co 550'(1100 to 1200'F)
Holdlng Ttne, Based on19.1 un (l ln,) or less
None
Holding Tlne, Based onUp to 5Q.8 nn (2 tn. )
l5 rninuces ninlur.lu,t hr. per 25.4 nro (tn. )
Holdlnq Tenperature
595 co 550'(1100 co 1200.F)
Nonolnal 9alI Thtcknes s
Over 50.8 rrun (2 tn )
2 hr. plus I5 minucesfor each addi clonal25.4 mra (tn.) over
50, 8 nm (Z in. )
?a qe :
Nores:
PWHT is not 'mandatory when:
1. The nominal waIl thickness is 19.l,ornm (t in. ) or Less,and
2 . a minimr::n preheat of 93 'C ( 2 Oo . F)nominal waII thickness of either25.4 Flyn (t in.).
is applj-ed when *-hebase metals exceei
*when it is iropracticar to pwHT at specif ied tenperat,ures, pwHTat }ower ternperatures over ronjer periods of tirne i spernrissable. See applicable Cod,e.
!: s -. -- cO -ar I p-15eE -o6 o o- o-La-Oo- t- > o.lt eeGoa C6lO.>L.ca-9eeCa - - t OO ob t t Lqo I foLGgco
I L! 0:-0n o o5 0s:5 PE-:= t6 C a o ! - e
eEcuvo9 -J< Cr d.-EE
lv{Ng<tO.OONn6NNhNNNNNnNmh\\\\\\\\\\ooooooooo6O6O(3O6oo6Nnn{6nn{66\o
oroor^rolr)(t656NFhbN6NNN
ltnroGsnrOl\OONNNIIAJNNNfVFOCtdO.ONn
NNnl-.TNNNNN
cto(fooo600QNTOgO.E6Olor\JNhsoooooooooo{tsO{€o'.@€o
N
ao'o'A.o-o-o-o.o-o-gr44Erd&EdgUL'(JU9O9UUo060600eoo
UIa
N^J\ONN€Nnaonn@h\\\\\\\\\\n€tstn6nN\\\\\\\\\\€lr)F\Oao€ls\O66r}C>r\.nO'ts6r{NtlF){Nhh96rO
olarOeooo
:383 83333OOGG€E€C€@€u66OeA696q
oaS'\-6€GO6
tlzfff:r--Tr-ri0aa6Oqo
EU
o
t
D9999qrc-NNNNCCCCCC .;sggggg
reEgdd
ii
lrlJlo
For{sr
I-tolrl3oHz(Ju.lF
:::::i:.:
FIG. ISINGLE MUARE
lrlr
I lG .t)DOUSLE SQUARE
{t
BUTT EUTT
FIG.Z5INGLE VEE BUTT
Fic-?DOUBLE VEE BUT]
Fr6.8DOUBLE U BUTT
FIG 3SING LE U BUTT
ctc 45INGLE J BUTT
5INGLE EEVEL BUTT
FIG.9DCUBI-E J BUTT
ltt/tlI\ I
ri-\t/t
-
DOUBLE BEVEL BUTT
G ROOVE DESIGN
3 -m il.?p.t/a^ n,/pll
is-\to\
SACKSIDE SHALL EEcouGED, cnodxD oRCl{IPPED TO EOUHD I.IETALBEFORE DEPO5ITINGFIRST PA95 ONBACK5IDE.
TYPICAL JOINT DE5IGN
oW4B3SUGGESTEDFoRMATFoRPRocEDUREQUALIFICATIoNREcoRD(PoR)(See QW-200.2, Section lX, ASME Boiler and Pressure Vessel Code)
Record Actual Conditions Used to Weld Test
WPS No.
Welding Process(es)Types (Manual, Automatic, Semi-Auto )
CompanyProcedure Qualification necor Date Januarv 29' 2001
JOTNTS (OW402)
E?ot8-l
E6o{o
Groove Design of Test CouPon
(For combination qualifications, the deposited weld metal thickness shall be recorded for each filler metal or process used )
BASE METALS (OW4o3)Material Spec. SA-106Type or Grad6 B
P-No. 1 P-No.
Thickness of Test CouponDiameter of Test CouponOther
0.375'6" (machined)
POSTWELDTemperature
HEAT TREATMENT (OW407)1125'F +l- 25"F
Time 2 Hr.
Other
FILLER METALS (OW4O4)SFA Specification 5,1 5.1
AWS Classification E6010 E701&'1
Filier Metal F-No. 3
Weld Metal Analysis A-No. IS izo of Fil I er M eta I 3/3 21,ll8l--------!13?1,Other
Weld MeLal Thickness T=0.125' T=0.25'
GAS (OW-408)Percent ComPosition
Gas(es) Mixture Flov/ Rate
Shielding
Trailing
Backing
N/A
POSTTTON (OW405)Position of Groove 5GWeld Progression (Uphlll, Downhill)OthBr
Uohill
ELECTRICAL CHARACTERI STI CS (ow40s)Current D.Q-
Polarity RevAmps, 6G90 Volts 1G20
Tungsten Electrode Size N/A
Other
PREHEAT (OW406)Preheat Temp, 50'Flnterpass Temp. 200"F Min. 550"FOther
Max.
TECHNTOUE (OW41o)
Travel Speed J-Bl.P.MString or Weave Bead Both
Oscillation N/AMultipass or Single Pass (per side) Multioass
Single or Multiple Electrodes SinqleOther
QW-483 (Back)
Tensile Test (QW.150)PQR No. 01S
SpecimenNo. Width (in) Thickness
(in)Area (in2)
UltimateTotal Load
tb
UltimateUnit Stress
psi
Type ofFailure &
Location
#5 0.739 0.353 0.261 1 8,1 90 69,700 D.P,M
#6 0.743 0.347 0.258 1 8,1 40 70,4 00 D,P.N4
Result-Satisfactory: YesMacro-Results
Gulded-Bend Tests (QW.1 60)
Toughness Tests (QW-170)
Fiilet-Wetd Test (eW-1 B0)
-
No _ Penetration into Parent Metal: Yes
Tvpe and Fiqure No. Res ult
Pass#1 Side Eend
#2 Slde Bend Pass
#3 Side Bend Pass
#4 Side Bend Pass
SpecimenNo.
NotchLocation
NotchType
TestTemp.
lmpactValues
Lateral Exp. Drop Weight
% Shear Mils BreakNo
Break
Other TestsType of TestDeposit AnalysisOther
Welder's Name Douq Bencharski Clock No, W-130S7 Stamp No.Tests conducted by: Alfor Metallurqic€l Laboratory fest f.lo Of -OA: -we certify that lhe stiatements in this record are correct and that the test welds were prepared, welded, and tested rn accordancewith the requirements of Section lX ofithe ASME Code.
Manufacturer
Date Januarv 29, 2001 By Terrv Wood(Detailofrecordoftestsareillustrativeonlyand'.y)
ALFOR METALLURGICAL COMPANY LTD.CONSULTING ENGINEERS
Grande Prairie Regional College10726 - 106 AvenueGrande Prairie, Alberta T8V 4C4
Results:
width:Thickness:Area:
Uitimate Load:Ultimate Tensile Strength :
Fracture Character:Fracture Location:
FILE #01-043
wPS #WE-02; PQR #01S
January 25,2001
Mtr,TAT TFST RF'PORT
Material Description: ASME SA-106, Grade B;NpS6 X 0.375" W.T. pipe; SMAW welded,E6010 Root + E7018-l Fill & Cap; PWHT condition,
Specimen Type: Reduced-section tensile, as per Figure QW-462.1(b) of the ASME Code;guided side bend, as per Figure eW-462.2 of the ASME Code.
Guided side bend samples 1,2,3, and 4: Pass Tests.
//,t'.,2rm/
Samnle 5
0,739 in.0.353 in.
0.261 sq. in.18 190 lb
69 700 psiDuctileParent
EDMONTON, ALBERTA T6E 5T4
Yours very truly,
ALFOR METALLURGICAL COMPANY LTD,
//,r- ',(-,zr'
/tr//>t/o / ' ,| ' ,,CHARLES. E. MOZESON, P. Eng.
Sample 6
0.743 in.0,347 in.
0.258 sq. in.18 140 lb
70 400 psiDuctileParent
6035 - 88 STREET, PHONE (780) 465-0s62
QW-483 SUGGESTED FORMAT FOR PROCEDURE QUALIFICATION RECORD (POR)
(See QW-200.2, Sec{ion lX, ASME Boiler and Pressure Vessel Code)Record Aclual Conditions Used to Weld Test Coupon
Company Name Woodland Enterprises, Box 718, Soirit River, Alberta T0H 3G0Procedure Qualification Record No. 02S Date January 29,2001WPS No. WE-02Welding Process(es) S.M.A.W.fypes (Manual, Automatic, Semi-Auto.) Manual
JOTNTS (OW402)
Groove Design of Test Coupon(For combination qualifications, the deoosited weld metal thickness shall be recorded for each filler metal or process used.)
BASE METALS (OW403)Material Spec. SA-106Type or Grade BP-No. P1 to P-No. P1
Thickness of Test CouponDiameter of Test CouponOther
0.s06'Pine 8' PlPtr
scH160
POSTWELDTemperature
HEAT TREATMENT (QW.4O7)1125"F +l-25"F
Time 2HrOther
FTLLER METALS (aW404)SFA Specification 5.1 5,1
AWS Classification E6010 E701&1Filler Metal F-No. F3 F4Weld Metal Analysis A-No. fSize of Filler Metal 3/32'. 1/8' 118'.114'Other
Weld Metal Thickness T=0.125" 0.781'
GAS (OW-408)Percent Composition
Gas(es) Mixture Flow Rate
N/AShielding
Trailing
POSTTTON (OW40s)Position of Groove 5GWeld Progression (Uphill, Downhill) UphillOther
ELECTRICAL CHARACTERTSTICS (OW-409)Cunent D.CPolarity RevAmps. 90-180 Volts 10-24Tungsten Electrode Size N/AOther
PREHEAT (OW406)PreheatTemp. 50"Flnterpass Temp. 200"F Min. 550"F Max.Other
TECHNTQUE (OW41o)Travel Speed 2-8l.P.M.String or Weave Bead !o'!hOscillation N/AMultipass or Single Pass (per side) MultioassSingle or Multiple Electrodes SinqleOther
QW483 (Back)
Tensile Test (QW'150)
PQR No. 02S
Fillet-Weld Test (QW-1 80)
Penetration into Parent Metal: Yes -
No
-Result-Satisfactory: Yes
UltimateUnit Stress
psi
Guided-Bend Tests (QW'1 60)
Toughnsss Tests (QW-170)
Lateral ExP. Drop Weight
SpecimenNo.
NotchLocation
NotchType
TestTemp.
lmpactValues
7o Shear Mils BreakNo.
Break
Macro-Results
Other Tests
Type of TestDeposit AnalYsis
Other
Welder's Name Douq Bencharski Clock No' W-13057 Stamp No'
Tests conducteo by: RttorJGGiilqi"tt Laboratory Test No 01-043
we certify that the statemiG in this record are *rrEtil-G"t tnu test welds were prepared, welded, and tested in accordance
with the requirements of Section lX of the ASME Code'
Manufacturer
Date Januarv 29.2001
(Detail of record of tests are illustrative only and
By Terrv Wood
,;;ffie and number of test required by the code.)
t
ALFOR
Grande Prairie Regional10726 - 106 AvenueGrande Prairie, Albeta
FILE #01-043
WPS #WE-02; PQR #02S
January 25,2001
MtrT I TFST RFPORT
METALLURGICAL COMPANY LTD.CONSULTING ENGINEERS
College
T8V 4C4
Material Description: ASME SA-106, Grade B; NPS8 X 0'906" W'T' pipe; SMAW weided;
E6010 Root + E7018-1 Fill & Cap; PWHT condition'
Specimen Type: Reduced-section tensile, as per Figure QW-462'1(b) of the ASME Code;
guidedsidebend,aSperFigureQw-462.2oftheASMECode.
Results:
width:Thickness:Area:Ultimate Load:Ultimate Tensile Strength:Fracture Character:Fracture Location:
Samfle 5
0.733 in.0.831 in.
0.609 sq. in.43 7001b71 700 psi
DuctileParent
-Sample 6
0.754 in.0.873 in.
0.658 sq. in.47 r50lb71 600 psi
DuctileParent
Guided side bend samples 1,2,3, and 4: Pass Tests'
/c- \
Yours very trulY,
ALFOR METALLURGICAL COMPANY LTD.
n,/z^,L'a//(4/a /CHARLES . E. MOZESON, P. Eng'
22/ bd!
Qw.4s3SUGGESTEDFoRMATFoRPRoGEDUREQUALIFICATIoNREcoRD(PoR)- 1a;" OW-200.2' Section lX, ASME Boiler and Pressure Vessel Code)
Welding Process(es)Types (Manual, Automatic, Semi-Auto')
Groove Design ofTest CouPon
weld metal thickness
POSTWELD HEAT TREATMENT (OW4O7)
Temperature 1125"F +l'25"FBASE METALS (OW403)Material Spec. SA-333 SA350
Type or Grade 6 LF2 . .
P-No. P1 - G1 P-No' P1 - G2
Thickness of Test CouPon
Diameter of Test Coupon - SCH 80 Mach' 4'
GAS (OW-408)Percent ComPositionFTLLER METALS (4w404)
SFA Specificailon 5.1 5'1
AWS Classification E6010 E701&1
Filler Metal F-No' gWeld Metal AnalYsis A'No' ISize of Filler Metal 3/32', 1/8' 3/32'' 1/8'
ELECTRICAL CHARACTERISTICS (OW-40e)
Cunent D.C.Polarity Bevemps.- OOg0 Volts 1G20
Position of Groove 5G
Weld Progression (Uphill' Downhill) Uohill
TECHNIQUE (OW410)Travel SPeed 2-8l.P.M'String or Weave Bead Both
Oscillation -N/AMultipass or Single Pass (per side) Multioass
Single or MultiPle Eleclrodes
ProheatTemp. 50"Flnterpass Temp. 200"F Min' 550'F Max.
Qw{83 (Back)
Tensile Test (QW-150)PQR No. 03S
Guided-Bend Tests (QW-l 60)
Tvoe and Fioure No. Result
Toughness Tests (QW-l 70) (See Attached)
SpecimenNo.
NotchLocation
NotchType
TestTemp.
lmpactValues
Lateral Exp. Drop Weight
% Shear Mils BreakNo.
Break
Result-Satisfactory: Yes
Fillst-Weld Test (QW-1 80)
Penetration into Parent Melal: Yes
Macro-Results_No-
Other TestsType of TestDeposit AnalysisOther
Weldeis Name Douq Bencharski Clock No. W{3052 Stamp No.
Tests conducted by: Alfor Metalluroical Laboratory Test No. 01-043We certify that the Stiatements in this record are correct and that the test welds were prepared, welded, and tested in accordance
with the requirements of Section lX of the ASME Code.
Manufacturer Woodland Enterorises. Box 718, Spirit River, Alberta TOH 3G0
Date Januarv 29,2001 By Terrv Wood
(Detail of record of tests are illustrative only and may be modifled to conform to the type and number of test required by the Code.)
Grande Prairie Regional College
10726 - 106 Avenue
Grande Prairie, Alberta T8V 4C4
ALFOR METALLURGICAL COMPANY LTD.CONSULTING ENGINEERS
FILE #01-043
WPS #wE-02; PQR #03S
January 25,200I
Material Description: ASME SA-333, Grade 6 to sA-350, Grade LF2; NPS4 X0'249" W'T';
SMAWwelded;E6010Root*E7018-lFill⋒PWHTcondition.
specimen Type: Charpy V-notch 0.221 inch (5.61 mm)-sized weld zone and heat-affected zone.i*pu"tspecimen,aSperPartUG-84oftheASMECode'
Testing Temperature: -50 F.
Results: weld zone : 39,26,37 ft-lb;
SA-333 Heat-affected zone: 49,63,72 ft-lb;
SA-350 Heat-affected zone: 23,27,34 ft-lb'
L/z.-
Yours very trulY,
ALFOR METALLURCICAL COMPANY LTD'
/) /,,_ _ .
L4'r />;/o /
CHARLES E. MOZESON, P' Eng'
'.- V7/ >(4 /
6035 . 88 STREET, EDMONTON, ALBERTAT6E 5T4 PHONE (780) 465-0562
QW-483 SUGGESTED FORMAT FOR PROCEDURE QUALIFICATIoN RECORD (POR)
'(SeeOW-200.2,SectionlX,ASMEBoilerandPressureVesselCode)Record Actual Conditions Used to Weld Test
company Name Woodland Enterorises. Box 718, Spirit River. Alberta ToH 3G0
Procedure Qualification necotO flo. OaS Date Januarv 29 2001
WPS No. WE-02Welding Process(es) S.M.A.W.Types (Manual, Automatic, Semi-Auto.) Manual
JOTNTS (OW-402)
Groove Design of Test CouPon
(Forcombinationqualifications,thedepositedweldmetaltnic
BASE METALS (OW.4O3)
Material Spec. SA-333 SA350Type or GradeP-No. Pl - Gl P-No. Pl - G2
Thickness ofTest Coupon 0.5'Diameter of Test Coupon B" SCH B0
Other
POSTWELD HEAT TREATMENT (OW4O7)
Temperature 1125"F +l-25"FTime 2fr.Other
FILLER METALSSFA Specification
(ow404)sl 5.1
AWS ClassificationFiller Metal F-No.
F6010 E701&'l
Weld Metal Analysis A-No. ISize of Filler Met:al 3/32", 1/8" 1/8'. 5/32'
Other
Weld Metal Thickness T=0.125' 0.375'
GAS (OW408)Percent ComPosition
Gas(es) Mixture Flow Rate
Shielding N/A
Trailing
POSTTTON (OW405)Position of Groove 5GWeld Progression (Uphill,Other
Downhill) Uohill
ELECTRICAL cHARACTERISTIcS (ow4os)Cunent D-CPolarity @Amps. 6G90 Volts 10-20
Tungsten Electrode Size $Other
PREHEAT (OW406)PreheatTemp. 50"Flnterpass Temp. 200'F Min. 550"F Max.
Other
TECHNIQUETravel Speed
(ow410)2 - 8 t.P.M.
String or Weave Bead Rnth
Oscillation N/AMultipass or Single Pass (per side) -Ugl!j-Dass.-Single or Multiple Elecfodes Sinqle
Other
QW483 (Back)
Tensile Test (QW-150)
PQR No. 04S
SpecimenNo. Width (in) Thickness
(in)Area (in2)
UltimateTotal Load
lb
UltimatoUnit Stress
psi
Type ofFailure &
Location
Guided-Bend Tests (QW-1 60)
Tvpe and Fiqure No. Result
Toughness Tests (QW-170) (See Attached)
SpecimenNo.
NotchLocation
NotchType
TestTemp.
lmpactValues
Lateral Exp. Drop Weight
% Shear Mils BreakNO
B reak
Result-Satisfactory: YesMacro-Results
Flllet-Weld Test (QW-1 80)
No Penetration into Parent Metal: Yes No
Other TestsType of TestDeposit AnalysisOther
Welder's Name Douq Bencharski Clock No w-13057 Stamp NoTests conducted by: Alfor Metalluroical Laboratory Test No. 01 -043
We certify that the stalements in this record are correct and that the test welds were prepared, welded, and tested in accordancewith the requirements of Section lX of the ASME Code.
Manufacturer Woodland Enterprises, Box 718, Spirit River, Alberra T0H 3GO
Date Januarv 29,2001 By Terrv Wood(Delail ol record of tests are illustrative only and may be modified to conform to the type and number of test required oy tne Coce. /
ALFOR METALLURGICAL COMPANY LTD.CONSULTING ENGINEERS
CI-{ARPY V-NOTCFI JMPACT TF'ST RFSIlT TS
Material Description: ASME SA-333, Grade 6 to SA-350, Grade LF2; NpS8 X 0.500" W.T.,SMAW welded; 86010 Root * 87018-1 Filt & Cap; pWHT condition
Specimen Type: Chatpy V-notch full-sized weld zone and heat-affected zone impacr specimcn,as per Part UG-84 of the ASME Code.
Testing Temperature: -50 F,
Results:Weld zone: 38, 33, 25 ft-lb;
SA-333 Heat-affected zone: 52, 8l ,74 ft-lb;
SA-350 Heat-affected zone: 68, 55, 61 ft-ib.
Grande Prairie Regional Coliege10726 - 106 AvenueGrande Prairie, Alberta T8V 4C4
Uaz" 7| 2e I
FILE #01-043
WPS #WE-02; PQR #0aS
January 25,2001
Yours very truly,
ALFOR METALLURGICAL COMPANY LTD.-//)/.1 ',(-4'-\ -
'
t />;/'01 . i
CHARLES E. MOZESON, P. Eng.
6035. 88 STREET, EDMONTON, ALBERTA T6E 5T4 PHONE (780) 46s-0s62
QW483 SUGGESTED FORMAT FOR PROCEDURE OUALIFICATION RECORD (POR)
(See QW-200,2, Section lX, ASME Boiler and Pressuro Vessel Code)
Record Actual Conditions Used to Weld Test Cou
Company Name Woodland Enterprises, Box 7.18, Spirit River, Alberta ToH 3G0
Procedure Qualification nucoto tlo. O5S Date Januarv 29' 2001
WPS No. WE-02Welding Process(es)Types (Manual, Automatic, Semi'Auto.) Manual
JOTNTS (OW402)
Groove Design of Test CouPon(For combination qualifications, the deposited weld metal thickness shall be recorded for each filler metal o_LPl99!l! il99:l
BASE METALSMaterial Spec.Type or Grade
(ow403)sA-333 SA350
LF2P-No. P1 - G1 P-No. rt -btThickness ofTest Coupon 0.5'Diameter of Test Coupon B' SCH B0
Other
POSTWELD HEAT TREATMENT (OW-407)
Temperature 1125.F +l- ?5"FTime 2Hr.Other
FTLLER METALS (OW4o4)SFA Specification s.1 5.1
AWS Classification E6010 E701&1Filler Metial F-No, 3
Weld Metal Analysis A-No. fSize of Filler Metal 3/32', 1/8" 118',5132'
Other
Weld Metal Thickness T=0.125" 0.375'
GAS (QW4o8)Percent ComPosltion
Gas(es) Mixture Flow Rate
N/AShlelding
Trailing
POSTTTON (OW4o5)Position of Groove 5GWeld Progression (Uphill, Downhill) Uohill
Other
ELECTRICAL oHARACTERISTICS (OW4o9)
Cunont D.QPolarity Rev
Amps. 60-90 Volts 10-20
Tungsten Electrode Size N/A
Othor
PREHEAT (OW406)Preheat Temp. 50"Flnterpass Temp.Other
200'F Min. 550"F Max.
TECHNTQUE (OW-410)
Travel Speed 2-8l.P.MString or Weave BoadOscillation N/A
Both
Multipass or Single Pass (per side) MultipassSingle or Multiple Electrodes SinoleOthor
QW-483 (Back)
Tensile Test (QW'150)PQR No. 055
Guided-Bend Tests (QW'1 60)
Tvpe and Fiqure No' Res u lt
Toughness Tests (QW-170) (See Attached)
SpecimenNo.
NotchLocation
NotchType
TestTemp.
lmpactValues
Lateral Exp. Drop Weight
% Shear Mils B reakNo.
Break
Fillet-weld Test (QW-l Bo)
Result-Satisfactory:Macro-Results
Yes
-
No Penetration into Parent Metal: Yes
Other Tests
Type of Test Vickers Hardness Test (See attached)
Deposit AnalysisOther
Welder's Name Douq Bencharski Clock No. W'13057 Stamp No
Tests conducted by: Alfor Metallurqical Laboratory Test No, 01-043
We certify that the statemenG in this record are correct and that the test welds were prepared, welded, and lested in accoroancewith the requirements of Section lX of the ASME Code.
Manufacturer Woodland Enterprises, Box 718, Soirit River, Alberta T0H 3G0
Date Januarv 29, 2001 By Terrv Wood
(Detail of record of tests are illustrative only and may be modified to conform to the type and number of test required by lne Cooe )
ALFOR METALLURGICAL COMPANY LTD.CONSULTING ENGINEERS
FILE #01-043
Grande Prairie Regional College
10726 - 106 AvenueGrande Prairie, Alberta T8V 4C4
wPS #wE-02; PQR #QfS
January 25,2001
Material Description: ASME SA-333, Grade 6 to SA-350, Grade LF2; NPSS X 0'500" S/ T';
SMAW welded; E6010 Root + E7018-l Fill & cap; PWHT condition
Vickers hardness testing at I kg mass (FIVI) was performed on a prepared cross-section of the
weldment, in accordan.i *itr ASTM E 92. All tests were performed at 1.5 mm below the surf-
ace; heat-affected zone tests were performed at 0'5 mm, 1.0 mm, and l '5 mm from the fusion
line. The results are tabulated below'
sA-333 sA*350
I ocation
ABC
DEF
HV1
187
196205186
185
152
T,ocation
G
HIJ
KL
T ,ocationHV1
180
t75172
161
t66169
Yours very trulY,
ALFOR METALLgRgICAL COMPANY LTD.
U/\-/f>;/o r
CHARLES E. MOZESON, P. Eng.
HVI
156
r55148
154
MNoP
a
Uz^-7, zM/
t/- Iast CaP Pass