deformation and strength characteristics of …concrete mix nsc hsc vhsc limestone coarse aggregate...

17
Assessment of Concrete Deformation and Failure Behavior during a Standard Fire Test and a Controlled Heating Rate Test Elin Jensen Department of Civil and Architectural Engineering ACI Spring Convention Kansas City, MO April 12, 2015

Upload: others

Post on 08-Aug-2020

2 views

Category:

Documents


0 download

TRANSCRIPT

Page 1: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Assessment of Concrete Deformation and Failure Behavior during a

Standard Fire Test and a Controlled Heating Rate Test

Elin Jensen

Department of Civil and Architectural Engineering

ACI Spring Convention

Kansas City, MO

April 12, 2015

Page 2: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Normal and High Strength Concrete Column Behavior

2

Kodur, V.K.R. Fire resistance design guidelines for high strength concrete columns. NRCC-46116 or ASCE/SFPE Specialty Conference of Design Structures for Fire and JFPE, Baltimore, MD, October 2003, pp. 1-11

Page 3: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Observations from Column Fire Testing

• The failure of the RC column is governed by the strength of the concrete

• Concrete carries an increasing portion of the applied column load as the steel temperature increases resulting in yielding and decreasing strength.

• The concrete strength also decreases with temperature

• The fire resistance decreases with increasing load intensity (loss of strength is higher in HSC than in NSC).

3

Page 4: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Motivation

4

0

200

400

600

800

1000

0 5 10 15

Tem

per

atu

re (°

C)

Time (hrs)

• How comparable are concrete behaviors observed from simulated controlled heating rate fire tests to that of concrete behavior in standard fire tests?

0

200

400

600

800

1000

1200

1400

0 2 4 6 8

Tem

per

atu

re (

°C)

Time (hrs)

ASTM E119 Standard Fire Curve

Page 5: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Concrete Mix NSC HSC VHSC

Limestone Coarse Aggregate (kg/m3) 1032 785 787

Limestone Fine Aggregate (kg/m3) 795 880 859

Limestone Intermediate Aggregate (kg/m3) - 349 288

Type 1 Cement (kg/m3) 203 259 262

Slag Cement (kg/m3) 110 146 141

Mid-Range Water Reducer (Super P) (L) 0.95 1.2 1.2

Water (kg/m3) 133 114.5 105

Water/Cementitious Materials Ratio 0.43 0.28 0.26

Compressive Strength (MPa)

28 days 51.5 63.4 90.0

At Time of Testing 52.5 77.5 107

5

Specimens around 80-87% internal RH prior to testingVHSC: conditioning at 45C

Specimens: 100 mm by 100 mm cross section area (length 450 & 900 mm)

Page 6: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Test Setup

6

Loaded Beam

Unloaded beam withembedded Thermocouples

Volume Stable Mullite Tubes

Ram

Base

Page 7: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Testing Procedure

• Specimen Preparation

• Loaded Prism

• Free Expansion Prism

• Specimen Loaded to the Predetermined Load

• Thermal Profile Started

• Sustained Load During the Cooling Phase

7

Specimen Failure at 740°C

Page 8: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Temperature Development in Standard Fire Test

8

0

100

200

300

400

500

600

700

800

900

0.0 0.5 1.0 1.5 2.0 2.5 3.0 3.5

Tem

per

atu

re (

oC

)

Time (hrs)

Core Surface Quarter

Page 9: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Temperature Development in Controlled Heating Rate Test

9

0

100

200

300

400

500

600

700

0 5 10 15 20 25 30

Tem

per

atu

re (o

C)

Time (hrs)Core Quarter Surface Environmental

Page 10: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Total Deformation

• Total deformation of concrete is expressed as the sum of four strain components as follows:

𝜀 = 𝜀𝑡ℎ 𝑇 + 𝜀𝑡𝜎 𝜎, 𝑇 + 𝜀𝑐𝑟 𝜎, 𝑇, 𝑡 + 𝜀𝑡𝑟 𝜎, 𝑇

• Components of Total Strain

• Thermal Strain (𝜀𝑡ℎ)

• Stress Related Strain (𝜀𝑡𝜎)

• Creep Strain (𝜀𝑐𝑟)

• Transient Strain (𝜀𝑡𝑟)

10

Page 11: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Total Strain Curves – Controlled Heating Rate

11

-3.5

-3

-2.5

-2

-1.5

-1

-0.5

0

0.5

0 100 200 300 400 500 600 700 800

% T

ota

l Str

ain

Temperature (oC)

α = 0.167 (52.5 MPa) α = 0.330 (52.5 MPa) α = 0.500 (52.5 MPa)

α = 0.167 (77.5 MPa) α = 0.330 (77.5 MPa) α = 0.500 (77.5 MPa)

*

*

* Specimen Failure

Page 12: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Total Strain ComparisonStandard Fire and Controlled Heating

12

-2

-1.5

-1

-0.5

0

0.5

0 100 200 300 400 500 600 700 800

% T

ota

l Str

ain

Temperature (oC)

ASTM, α = 0.250 ASTM, α = 0.167 (1) ASTM, α = 0.167 (2)

600°C, α = 0.167(NSF) 800°C, α = 0.167(NSF)

* Specimen Failure

NSF = Non-Standard Fire

*

*

*

Page 13: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

During and After Standard Fire Test

13

Specimen Failure for initial load level = 0.33

Core temperatures less than 150°C

Spalling near110 C core temperature

Specimen behavior similar at = 0.167 and = 0.25

Longitudinal Crack develops during test(450 - 500°C)

Page 14: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Total Strain ComparisonStandard Fire and Controlled Heating

14

-2

-1.5

-1

-0.5

0

0.5

0 100 200 300 400 500 600 700 800

% T

ota

l Str

ain

Temperature (oC)

ASTM, α = 0.250 ASTM, α = 0.167 (1) ASTM, α = 0.167 (2)

600°C, α = 0.167(NSF) 800°C, α = 0.167(NSF)

* Specimen Failure

NSF = Non-Standard Fire

*

*

*

20% Spalling

0.33

controlled

Page 15: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Observations

• The deformation and failure behavior was similar for concrete prisms when load intensity and average core temperature was accounted for.

• Results indicated that deformations exceeding ≈ 1%, whether they occur during heating or cooling, are expected to cause an unstable ‘runaway’ failure.

15

Page 16: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Acknowledgements

• National Science Foundation Award #0747775

• Center for Innovative Materials Research (CIMR) at Lawrence Technological University

• Assistance During Experimental Research From:

• Brittany Schuel, Mishi Joshi, Daniel Ziemba, Carl Durden

16

Page 17: DEFORMATION AND STRENGTH CHARACTERISTICS OF …Concrete Mix NSC HSC VHSC Limestone Coarse Aggregate (kg/m3) 1032 785 787 Limestone Fine Aggregate (kg/m3) 795 880 859 Limestone Intermediate

Thank you!

17